Anisotropic multifunctional carbon-based wave-absorbing aerogel as well as preparation method and application thereof

By combining graphene oxide with carbon oxide nanotubes, anisotropic multifunctional carbon-based aerogel is prepared, which solves the problem of insufficient heat resistance of carbon-based aerogels in high temperature and flammable environments, and achieves light quality , elastic, thermal insulation, flame retardant and low-cost versatility, suitable for aerospace applications.

CN118929648APending Publication Date: 2024-11-12BEIJING UNIV OF CHEM TECH

Patent Information

Application Number
CN202411123467.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing carbon-based absorbent materials have insufficient heat resistance in high temperature and flammable environments, and are highly versatile and cost-effective, making it difficult to meet the needs of lightweight, elastic, heat insulation, flame retardant and low-cost.

Method used

The anisotropic multifunctional carbon-based aerogel is prepared by combining graphene oxide with carbon oxide nanotubes, and anisotropic multifunctional carbon-based aerogels are prepared through directional freezing and heat treatment. Polyphosphazene is used to improve flame retardant performance, and the structure is optimized through ultrasonic and vacuum freeze-drying to achieve Low-cost industrial production.

Benefits of technology

The prepared aerogel has excellent flame retardant and heat insulation properties, strong reflection loss, wide effective absorption bandwidth, and is suitable for aerospace applications, with low cost and simple process, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929648A_ABST
    Figure CN118929648A_ABST
Patent Text Reader

Abstract

The invention provides anisotropic multifunctional carbon-based wave-absorbing aerogel as well as a preparation method and application thereof, and belongs to the technical field of wave-absorbing materials. The preparation method of the anisotropic multifunctional carbon-based wave-absorbing aerogel comprises the following steps: mixing a graphene oxide solution with a carbon oxide tube to obtain a mixed solution A; mixing the mixed solution A with a polyphosphazene ethanol solution, adding deionized water, and performing ultrasonic treatment to obtain a mixed solution B; carrying out directional freezing and vacuum freeze drying on the mixed solution B to obtain GCP aerogel; and carrying out heat treatment on the GCP aerogel to obtain the anisotropic multifunctional carbon-based wave-absorbing aerogel. The RCP aerogel prepared by the preparation method disclosed by the invention shows excellent wave absorbing performance in a frequency band of 2-18GHz, the maximum reflection loss parallel to a freezing direction is-61.5 dB, and the effective absorption bandwidth is 6.6 GHz; the maximum reflection loss perpendicular to the freezing direction is-29.4 dB, and the effective absorption bandwidth is 8.96 GHz.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wave-absorbing materials, and in particular relates to an anisotropic multifunctional carbon-based wave-absorbing aerogel and a preparation method and application thereof. Background Art

[0002] With the rapid development of information technology, electromagnetic waves play an increasingly important role in modern society, especially in the fields of wireless communication and radar detection. However, electromagnetic waves also bring about problems such as electromagnetic radiation pollution and electromagnetic interference that cannot be ignored, especially in specific environments such as aerospace, military defense and power transmission. Therefore, it is very important to develop efficient electromagnetic wave absorbing materials.

[0003] The current electromagnetic wave absorbing materials are mainly nanopowders formed by magnetic metals and their composite materials. The combination of magnetic components and dielectric materials not only optimizes impedance matching, but also enhances the ability to coordinate the loss of electromagnetic waves. However, this type of absorbing material usually has a high filling amount in the matrix, which leads to a high density and easy agglomeration of the material. In addition, with the advancement of technology, the requirements of modern society for materials have exceeded the single absorbing function. Especially in extreme environments such as high temperature and flammability, materials also need to have additional properties such as heat insulation and flame retardancy to ensure their absorbing ability and safety. Therefore, the development of efficient electromagnetic wave absorbing materials with multiple properties has become an urgent need.

[0004] Constructing a three-dimensional porous structure can effectively solve the above problems. The rich pore structure can optimize the impedance matching of the material while reducing the density of the material itself, so that most electromagnetic waves can enter the material and be reflected and scattered multiple times in the pores until they are completely absorbed. In addition, this three-dimensional porous structure gives the material ultra-lightness, excellent mechanical properties and fatigue resistance, making it suitable for complex aerospace applications that are sensitive to weight. Recently, aerogels with a three-dimensional porous structure based on reduced graphene oxide have been widely studied. Reduced graphene oxide has a large specific surface area and excellent electrical properties, which can produce strong conduction losses to electromagnetic waves. At the same time, the rich lattice defects and residual oxygen-containing functional groups on reduced graphene oxide can act as polarization centers to produce polarization responses to electromagnetic waves. However, the heat resistance of the carbon component is limited, and the research on high thermal stability carbon-based absorbing materials is insufficient, resulting in a limited application range of carbon-based absorbing materials.

[0005] A multifunctional absorbing aerogel and a preparation method thereof disclosed in China Invention Patent Publication No. CN 114350159 A can realize multifunctionality of absorbing, high strength and high elasticity, heat insulation and hydrophobicity through multi-level structural design and precise compounding of multiple components, but its reflection loss is relatively weak; A multifunctional absorbing aerogel and a preparation method and application thereof disclosed in China Invention Patent Publication No. CN 117209835 A has good resilience and hydrophobicity, and its 3D structure is also conducive to increasing interface polarization and multiple scattering, and has excellent electromagnetic wave dissipation capacity, but it has problems such as narrow absorption band, high cost and complex preparation process.

[0006] Therefore, there is an urgent need for a multifunctional carbon-based microwave-absorbing aerogel that is lightweight, elastic, heat-insulating, flame-retardant, low-cost, and easy to mass-produce. Summary of the invention

[0007] In view of this, the purpose of the present invention is to provide an anisotropic multifunctional carbon-based absorbing aerogel and a preparation method and application thereof. The aerogel prepared by the present invention presents an anisotropic structure, strong reflection loss, effective absorption bandwidth, a three-dimensional porous structure and a high phosphorus and nitrogen content, and exhibits excellent flame retardant and heat insulation properties. The preparation process is simple, the cost is low, and it is suitable for industrial production.

[0008] In order to achieve the above object, the present invention provides the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing an anisotropic multifunctional carbon-based absorbing aerogel, comprising the following preparation steps:

[0010] 1) mixing a graphene oxide solution and an oxidized carbon tube to obtain a mixed solution A;

[0011] 2) mixing the mixed solution A with the polyphosphazene ethanol solution and adding deionized water, followed by ultrasonic treatment to obtain a mixed solution B;

[0012] 3) subjecting the mixed solution B to directional freezing and vacuum freeze drying to obtain GCP aerogel;

[0013] 4) The GCP aerogel is subjected to heat treatment to obtain anisotropic multifunctional carbon-based wave-absorbing aerogel (RCP).

[0014] Graphene oxide / oxidized carbon nanotubes / hexachlorocyclotriphosphazene is simplified to "GCP"; Reduced graphene oxide / oxidized carbon nanotubes / hexachlorocyclotriphosphazene is simplified to "RCP".

[0015] By adopting the above technical scheme, in the present invention, graphene oxide and oxidized carbon nanotubes contain a large amount of hydroxyl, epoxy, carboxyl and carbonyl functional groups, which can be well dispersed in aqueous solution. Due to the interaction of van der Waals force, π-π stacking and hydrogen bonds, oxidized carbon nanotubes present a uniform dispersion state, and are closely attached to the graphene oxide sheet, avoiding the occurrence of agglomeration. After heat treatment, the graphene oxide and oxidized carbon nanotube skeletons are appropriately reduced, which improves the electron transmission capacity, thereby improving the conduction loss of the material to electromagnetic waves. In addition, the abundant lattice defects and residual oxygen-containing functional groups can be used as polarization centers to produce polarization responses to electromagnetic waves. At the same time, polyphosphazene is converted into phosphorus oxide compounds, enriching polar functional groups and improving the flame retardant properties of the material.

[0016] Preferably, the concentration of the graphene oxide solution in step 1) is 8-12 mg / mL.

[0017] Preferably, the concentration of the polyphosphazene ethanol solution in step 2) is 120-150 mg / mL.

[0018] Preferably, the mass ratio of graphene oxide, carbon oxide tubes and polyphosphazene in the mixed solution B of step 2) is 10:2:1.

[0019] By controlling the concentration of graphene oxide, the pore size of the aerogel can be effectively adjusted, thereby adjusting the dielectric parameters. By adjusting the concentration of graphene oxide, the impedance matching can be optimized, thereby achieving the effect of improving the absorption performance.

[0020] Preferably, in step 2), the mixing time is 30-40 min; the ultrasonic time is 40-60 min, and the ultrasonic power is 200 W.

[0021] Preferably, the concentration of graphene oxide in the mixed solution B in step 2) is 2-8 mg / mL.

[0022] Preferably, in step 3), the vacuum freeze drying temperature is -50°C, the time is 3 days, and the pressure is <10Pa.

[0023] Preferably, the heat treatment method in step 4) is under Ar atmosphere, with a treatment temperature of 400°C, a treatment time of 1h, a heating rate of 2°C / min, and a gas velocity of 100mL / min.

[0024] In a second aspect, the present invention provides an anisotropic multifunctional carbon-based absorbing aerogel prepared by the preparation method described above.

[0025] In a third aspect, the present invention provides an application of the above-mentioned anisotropic multifunctional carbon-based absorbing aerogel in the field of absorbing waves.

[0026] Contains at least the following beneficial technical effects:

[0027] The aerogel prepared by the present invention presents an anisotropic structure, with a honeycomb porous structure parallel to the freezing direction and a neat layered structure perpendicular to the freezing direction. This three-dimensional porous structure not only reduces the density of the material, but also optimizes the impedance matching, allowing most electromagnetic waves to penetrate deep into the material, undergo multiple reflections and scattering in the pores, and eventually be completely absorbed. The maximum reflection loss parallel to the freezing direction is -61.5dB, and the effective absorption bandwidth is 6.6GHz; the maximum reflection loss perpendicular to the freezing direction is -29.4dB, and the effective absorption bandwidth is 8.96GHz.

[0028] The aerogel prepared by the present invention has a three-dimensional porous structure and a high phosphorus and nitrogen content. The aerogel also exhibits excellent flame retardancy and heat insulation properties, and the thermal conductivity along the direction parallel to the freezing direction is as low as 20.6 mW m -1 K -1 , can continue to burn for 45 minutes under an alcohol lamp; the thermal conductivity along the direction perpendicular to the freezing direction is 26.2mW m -1 K -1 , can continue to burn for 31 minutes under an alcohol lamp. In addition, it also shows ultra-light (<6mg cm -3 ), excellent mechanical properties and fatigue resistance, making it very suitable for aerospace applications where material weight is extremely important.

[0029] The preparation process of the invention is simple, the cost is low and it is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The SEM (scanning electron microscope) images of the anisotropic multifunctional carbon-based absorbing aerogel obtained in Example 1, wherein (a) is a SEM image of the aerogel parallel to the freezing direction (longitudinal direction); (b) is a SEM image of the aerogel perpendicular to the freezing direction (transverse direction);

[0031] Figure 2 The XRD (X-ray diffraction) diagram of the anisotropic multifunctional carbon-based absorbing aerogel before and after heat treatment;

[0032] Figure 3 The mechanical properties of the anisotropic multifunctional carbon-based absorbing aerogel obtained in Example 1 are shown in Figure 1, wherein (a) is a compression stress-strain curve; (b) is a 300-cycle compression curve at 50% strain;

[0033] Figure 4 The thermal insulation and flame retardant performance diagram of the anisotropic multifunctional carbon-based absorbing aerogel obtained in Example 1, wherein (a) is the thermal conductivity of the aerogel as a whole, in the longitudinal direction, and in the transverse direction; (b) is a curve diagram of the change of the mass of the aerogel under an alcohol lamp over time;

[0034] Figure 5 The microwave absorption performance diagram of the anisotropic multifunctional carbon-based microwave-absorbing aerogel obtained in Example 1 along the longitudinal direction (a) and the transverse direction (b);

[0035] Figure 6 This is a comparison chart of the longitudinal microwave absorption performance of the anisotropic multifunctional carbon-based absorbing aerogel obtained in Examples 1-4. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The term "include" or "comprising" in the present invention is an open description containing the specified components or steps described, and other specified components or steps that will not be substantially affected.

[0038] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0039] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.

[0040] In the following examples, natural graphite flakes (-325 mesh) and hexachlorotripolyphosphazene were purchased from Alfa Aesar Chemical Co., Ltd., and multi-walled carbon nanotubes (purity 95%, length less than 10 μm, diameter 20 nm) were purchased from Jiangsu Pioneer Nanomaterials Technology Co., Ltd.

[0041] Graphene oxide is synthesized by the following method: 3g graphite powder, 1.5g sodium nitrate are added to 70mL concentrated sulfuric acid in an ice-water bath, stirred and mixed evenly, 9g potassium permanganate is slowly added several times, stirred evenly, and after all are added, the temperature is raised to 35°C and stirred for 30min-1h, 150mL water is slowly added and the temperature is raised to 80°C for reaction for 15min. After cooling, pour into 500mL deionized water, add 15mL hydrogen peroxide (30%) and let stand, remove the upper liquid, filter the lower liquid with a Buchner funnel, wash with acid water several times, disperse the filter cake in 400mL water, centrifuge at 4000rmp to obtain the suspension, and centrifuge the suspension at 10000rmp to obtain the precipitate. The precipitate is well dispersed and dialyzed for one week with a dialysis bag to obtain a graphene oxide solution.

[0042] Oxidized carbon nanotubes were synthesized by the following method: First, 2.0 g of carbon nanotubes were weighed and laid flat in a porcelain boat, and then calcined at 430 ° C for 1 h in air. The obtained sample was poured into a round-bottom flask (with a magnet added), 60 mL of nitric acid was weighed and slowly added, and then 180 mL of concentrated sulfuric acid was weighed and slowly added, and the round-bottom flask was fixed in a constant temperature bath (60 ° C) and stirred for 6 h. The reaction mixture was slowly added to 1.5 L of deionized water, and allowed to stand overnight. After the solid and liquid layers were separated, the lower layer of solid was taken and washed by centrifugation with dilute hydrochloric acid and deionized water for 3 times to obtain a solid. The solid was then dispersed in deionized water for ultrasonic dispersion and dialyzed for one week, and finally vacuum freeze-dried to obtain oxidized carbon nanotubes.

[0043] Example 1

[0044] This embodiment provides an anisotropic multifunctional carbon-based microwave absorbing aerogel, and the preparation method thereof is as follows:

[0045] 1) Prepare a mixed solution with a graphene oxide concentration of 4 mg / mL: measure 1.68 mL of 9.5 mg / mL graphene oxide solution in a beaker and add a magnet; weigh 3.2 g of carbon oxide tubes and add them to the beaker to obtain a mixed solution A;

[0046] 2) Then, 11 μL of a 150 mg / mL polyphosphazene ethanol solution was measured and dripped into the mixed solution A, and finally 2.309 mL of deionized water was added and magnetically stirred for 35 min, and then transferred to an ultrasonic tank and ultrasonicated at a power of 200 W for 50 min to obtain a mixed solution B;

[0047] 3) The mixed solution B was transferred to the assembled polytetrafluoroethylene mold for directional freezing, and after the freezing was completed, it was transferred to a freeze dryer and vacuum dried at -50°C and <10Pa for 3 days to obtain GCP aerogel;

[0048] 4) The GCP aerogel was transferred to a tubular furnace and heat treated at 400 °C for 1 h under Ar atmosphere to obtain anisotropic multifunctional carbon-based microwave absorbing aerogel (RCP).

[0049] Example 2

[0050] The preparation method of this embodiment is the same as that of embodiment 1, except that the concentration of graphene oxide in the mixed solution is 2 mg / mL, the carbon oxide tube is 1.6 g, and the polyphosphazene ethanol solution is 5 μL.

[0051] Example 3

[0052] The preparation method of this embodiment is the same as that of embodiment 1, except that the concentration of graphene oxide in the mixed solution is 6 mg / mL, the carbon oxide tube is 4.8 g, and the polyphosphazene ethanol solution is 16 μL.

[0053] Example 4

[0054] The preparation method of this embodiment is the same as that of embodiment 1, except that the concentration of graphene oxide in the mixed solution is 8 mg / mL, the carbon oxide tube is 6.4 g, and the polyphosphazene ethanol solution is 21 μL.

[0055] Experimental Example 1

[0056] The microscopic morphology of the RCP aerogel prepared in Example 1 was characterized and observed by scanning electron microscopy (SEM, Regulus 8240). A small piece of aerogel sample was cut along the direction parallel to the freezing direction and perpendicular to the freezing direction and glued to the surface of the aerogel for testing. The measured SEM images are shown in FIG. Figure 1 As shown, it presents a honeycomb porous structure parallel to the freezing direction and a neat layered structure perpendicular to the freezing direction.

[0057] X-ray diffraction was measured by a Bruker D2 Phaser instrument. The XRD patterns of the GCP aerogel and RCP aerogel prepared in Example 1 are shown in FIG. Figure 2 As shown, the diffraction peak at 2θ≈11° corresponds to the (001) crystal plane of graphene oxide, which suggests that the oxidized carbon tubes are uniformly loaded on the graphene oxide sheets without phase separation. After annealing, the (001) diffraction peak of graphene oxide disappears and turns into the (002) diffraction peak of reduced graphene oxide, indicating the effective reduction of graphene oxide.

[0058] Figure 3(a) is the compression stress-strain curve of the RCP aerogel in Example 1, and (b) is the compression cycle curve under the condition of 50% strain. The RCP aerogel can quickly recover its original morphology under 20%-80% strain, indicating that it has good resilience. After 300 cycles of compression, the RCP aerogel retains 72% of the maximum compressive strength, indicating that it has good cycle durability.

[0059] Figure 4 (a) and (b) are the thermal conductivity of the aerogel prepared in Example 1 along the longitudinal direction (parallel to the freezing direction) and transverse direction (perpendicular to the freezing direction) and the mass loss curve under an alcohol lamp. The RCP aerogel has good thermal insulation and flame retardant properties along the longitudinal direction, and the thermal conductivity is as low as 20.6 mW m -1 K -1 , can burn continuously for 45 minutes under alcohol lamp; the thermal conductivity along the transverse direction is 26.2mWm -1 K -1 , can continue to burn for 31 minutes under alcohol.

[0060] The microwave absorption performance of RCP aerogel along the longitudinal and transverse directions was tested by vector network analyzer (Agilent E5071C). Figure 5 As shown, the maximum reflection loss in the longitudinal direction is -61.5dB, and the effective absorption bandwidth is 6.6GHz; the maximum reflection loss in the transverse direction is -29.4dB, and the effective absorption bandwidth is 8.96GHz.

[0061] Figure 6 The figure is a comparison of the maximum reflection loss and effective absorption bandwidth of the RCP aerogels obtained in Examples 1-4 at different graphene oxide concentrations. With the increase of graphene oxide concentration, the longitudinal pore size of the RCP aerogel becomes more and more dense, and the corresponding electromagnetic wave absorption performance shows a trend of first getting better and then getting worse. Under the conditions of graphene oxide concentration of 4 mg / mL and 6 mg / mL, the RCP aerogel shows excellent electromagnetic wave absorption performance. The reason is that the appropriate pore size structure can effectively adjust the dielectric parameters of the RCP aerogel and optimize the impedance matching.

[0062] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for preparing anisotropic multifunctional carbon-based microwave absorbing aerogel, characterized in that: The method comprises the following preparation steps: 1) mixing a graphene oxide solution and an oxidized carbon tube to obtain a mixed solution A; 2) mixing the mixed solution A with the polyphosphazene ethanol solution and adding deionized water, and then ultrasonicating to obtain a mixed solution B; 3) subjecting the mixed solution B to directional freezing and vacuum freeze drying to obtain GCP aerogel; 4) The GCP aerogel is subjected to heat treatment to obtain anisotropic multifunctional carbon-based absorbing aerogel.

2. The preparation method according to claim 1, characterized in that: The concentration of the graphene oxide solution in step 1) is 8-12 mg / mL.

3. The preparation method according to claim 1, characterized in that: The concentration of the polyphosphazene ethanol solution in step 2) is 120-150 mg / mL.

4. The preparation method according to any one of claims 1 to 3, characterized in that The mass ratio of graphene oxide, carbon oxide tubes and polyphosphazene in the mixed solution B of step 2) is 10:2:

1.

5. The preparation method according to claim 1, characterized in that: In the step 2), the mixing time is 30-40 min; the ultrasonic time is 40-60 min, and the ultrasonic power is 200 W.

6. The preparation method according to claim 1, characterized in that: The concentration of graphene oxide in the mixed solution B of step 2) is 2-8 mg / mL.

7. The preparation method according to claim 1, characterized in that: In the step 3), the vacuum freeze drying temperature is -50°C, the time is 3 days, and the pressure is <10Pa.

8. The preparation method according to claim 1, characterized in that: The heat treatment method in step 4) is under Ar atmosphere, with a treatment temperature of 400° C., a treatment time of 1 h, a heating rate of 2° C. / min, and a gas velocity of 100 mL / min.

9. An anisotropic multifunctional carbon-based microwave absorbing aerogel, characterized in that: The compound is prepared by the preparation method described in any one of claims 1 to 3 or claims 5 to 8.

10. Application of the anisotropic multifunctional carbon-based absorbing aerogel according to claim 9 in the field of absorbing waves.

Citation Information

Patent Citations

  • Graphene-carbon nano tube composite all-carbon ultra-light elastic aerogel and preparation method thereof

    CN102674315A

  • Preparation method of graphene aerogel and graphene-carbon nanotube aerogel

    CN104401977A

  • Composition used for flame-retardant composite material, graphene flame-retardant foam and preparation method and application thereof

    CN105295959A

  • Flexible and self-supported graphene hybrid electrode and preparation method and application thereof

    CN107240511A

  • Graphene / carbon nanotube aerogel electromagnetic shielding composite fabric as well as preparation method and application thereof

    CN113386412A

Cited By

  • MnFe2O4 / GO wave-absorbing aerogel with directional aperture structure and preparation method of MnFe2O4 / GO wave-absorbing aerogel

    CN120364757A

  • MnFe2O4 / GO wave-absorbing aerogel with directional aperture structure and preparation method thereof

    CN120364757B

  • Preparation method of multi-layer graphene / polyimide composite aerogel with different pore diameters