Biomass carbon-based material as well as preparation method and application thereof

By using soluble salts such as straw and potassium hydroxide activated titanium modified biomass carbon-based materials as the positive electrode of zinc air battery, the problems of high cost and unstable activity of precious metal catalysts are solved, and efficient and stable electrochemical performance are achieved. Low-cost energy conversion device applications.

CN118929661APending Publication Date: 2024-11-12HENAN AGRICULTURAL UNIVERSITY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410999282.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The cathode catalysts of existing fuel cells and zinc-air batteries are expensive and unstable in performance. In particular, the scarcity of precious metal catalysts and the agglomeration of platinum nanoparticles lead to reduced activity and durability, making it difficult to promote and apply on a large scale.

Method used

Using straw as the main raw material, the pore-making process is activated by adding soluble iron salt, soluble zinc salt and potassium hydroxide to activate pore-making and calcining is obtained to obtain the precursor material. The soluble titanium salt is modified by hydrothermal method using the reinforcement method to prepare titanium modified plant The material carbon-based material serves as the positive electrode of the zinc-air battery.

Benefits of technology

It improves the structural and catalytic performance stability of biomass carbon-based materials, achieves high power density and discharge stability, reduces production costs, and has good application prospects for energy storage and conversion devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929661A_ABST
    Figure CN118929661A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of electrochemical catalyst synthesis and energy conversion devices, and particularly discloses a biomass carbon-based material and a preparation method and application thereof. According to the biomass carbon-based material, straw is used as a main raw material, soluble ferric salt, soluble zinc salt and potassium hydroxide are added for activation and pore forming, then high-temperature calcination is conducted, a precursor material is obtained, soluble titanium salt is used as an enhancer, the precursor material is modified through a hydrothermal method, and the titanium-modified biomass carbon-based material is obtained. The positive electrode can be used as a zinc-air battery. Researches show that the zinc-air battery based on the titanium modified biomass carbon-based material has relatively high power density and extremely high discharge stability, which indicates that the biomass carbon-based material has a good development prospect in the fields of energy storage and conversion devices such as the zinc-air battery and a fuel cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electrochemical catalyst synthesis and energy conversion devices, and specifically relates to a biomass carbon-based material and a preparation method and application thereof. Background Art

[0002] At present, the biggest obstacle for fuel cells and zinc-air batteries is the cathode catalyst, which directly affects the performance and life of fuel cells and zinc-air batteries. In addition, although the cathode catalysts of fuel cells and zinc-air batteries are used in different environments, most of the cathode catalysts can be used in both. Cathode catalysts can be roughly divided into precious metal catalysts and non-precious metal catalysts. The research on precious metal catalytic materials is mainly based on platinum (Pt), while the research on precious metals such as gold (Au), palladium (Pd), and iron (Ir) is relatively small. In theory, the activity and durability of pure platinum catalytic materials are guaranteed, but the cost of catalytic materials is unacceptable, so reducing the amount of platinum materials used is the focus and difficulty of platinum-based catalytic material research. Nano-sizing of platinum materials can expose more specific surface area (active interface) of platinum particles, that is, less platinum is needed to maintain the same activity. However, high specific surface area and high active crystal planes often mean that the size of platinum particles is reduced to a few nanometers, which will make platinum particles abnormally active and more prone to agglomeration, thereby reducing the specific surface area of ​​the material, which is manifested as a decrease in both the activity and durability of the catalytic material. Studies have shown that the interaction between the carrier and platinum nanoparticles can effectively alleviate the agglomeration of platinum nanoparticles and optimize the catalytic interface, so supported platinum-based catalytic materials have received great attention. Currently, the most widely used carriers are carbon carriers, such as carbon black, activated carbon, carbon nanotubes and graphene. From a cost perspective, due to the scarcity of precious metals, precious metal catalytic materials are expensive and not conducive to large-scale promotion and application, so non-precious metal catalytic materials also have important research value.

[0003] Biomass carbon-based materials are solid products synthesized from carbon-rich biomass through carbonization, pyrolysis, etc. They have good chemical inertness, heat resistance, electrical conductivity and thermal conductivity, and can ensure the stability of electrocatalysts and charge transfer efficiency. At the same time, biomass carbon-based materials have rich pore structures, large specific surface areas and a large number of oxygen-containing functional groups, which are beneficial to improving the rate of electrocatalytic reactions. Biomass carbon-based materials contain trace amounts of heteroatoms such as nitrogen and sulfur. After modification, the carbon substrate doped with metals and heteroatoms can provide active sites for releasing and adsorbing oxygen, respectively. In addition, the raw materials are cheap and easy to obtain, and the preparation process is simple. It is one of the ideal raw materials for biomass carbon-based electrocatalysts.

[0004] Chinese patent application CN115224291A (Zhengzhou University of Light Industry) discloses a hollow spherical iron (Fe) and nitrogen (N) co-doped porous carbon-based catalyst, using polystyrene as a template, iron salts, zinc salts, and nitrogen-containing heteroatom polymers as raw materials, and in-situ oxidative polymerization to obtain a polymer coating layer that chelates Fe atoms on the surface of the polystyrene sphere, followed by calcination and acid washing to obtain a Fe-N-HPCs-based high-efficiency zinc-air battery catalyst. Experiments show that the catalyst has a high open circuit voltage, power density, and stability in a 0.1M potassium hydroxide solution. In recent years, with the rapid development of agriculture, more and more straw waste has been generated, and burning straw will cause greater pollution to the surrounding environment. If the waste straw can be comprehensively recycled and used to prepare biomass carbon-based materials and produce carbon-based electrocatalysts, it will not only solve the problem of environmental pollution, but also realize the resource recycling of waste straw. Summary of the invention

[0005] The main technical problem solved by the present invention is to provide a biomass carbon-based material, which takes straw as the main raw material, adds soluble iron salt, soluble zinc salt and potassium hydroxide to activate and form pores, and then calcines at high temperature to obtain a precursor material, and uses a soluble titanium salt as a reinforcing agent to modify the precursor material by a hydrothermal method to obtain a titanium-modified biomass carbon-based material, which can be used as the positive electrode of a zinc-air battery.

[0006] Secondly, the present invention provides a method for preparing a biomass carbon-based material.

[0007] Again, the present invention provides an application of a biomass carbon-based material in the preparation of a zinc-air battery.

[0008] Finally, the present invention provides a zinc-air battery.

[0009] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0010] A biomass carbon-based material uses straw as a main raw material, adds soluble iron salt, soluble zinc salt and potassium hydroxide to activate and form pores, then calcines and carbonizes to obtain a precursor material, and then adds soluble titanium salt to heat to form a titanium dioxide surface modification layer to obtain the biomass carbon-based material.

[0011] As a preferred embodiment of the present invention, the straw includes but is not limited to corn straw and wheat straw.

[0012] As a preferred embodiment of the present invention, the soluble iron salt includes but is not limited to ferric chloride, ferric bromide, ferric sulfate, and ferric nitrate.

[0013] As a preferred embodiment of the present invention, the soluble zinc salt includes but is not limited to zinc chloride, zinc bromide, zinc nitrate, and zinc sulfate.

[0014] As a preferred embodiment of the present invention, the soluble titanium salt includes but is not limited to titanium tetrachloride and titanium sulfate.

[0015] As a preferred embodiment of the present invention, the activation pore making is: mixing straw powder with ferric chloride, zinc chloride, potassium hydroxide and water, activating the mixture at 50-80°C for 1-5 hours, and drying the mixture to form powder, preferably at 60°C for 2 hours.

[0016] As a preferred embodiment of the present invention, the calcination carbonization is as follows: in a protective atmosphere, the powder is heated to 800-1200°C for carbonization treatment for 1-5 hours. The heating rate is 5-15°C / min. Preferably, the carbonization treatment is carried out at 900°C for 2 hours, and the heating rate is 10°C / min.

[0017] As a preferred embodiment of the present invention, the hydrothermal reaction is: mixing the precursor material with titanium tetrachloride and water, and performing a hydrothermal reaction at 150-200° C. for 5-10 hours, preferably at 180° C. for 8 hours.

[0018] A method for preparing a biomass carbon-based material, the method comprising the following steps:

[0019] (1) mixing straw powder with soluble iron salt, soluble zinc salt, potassium hydroxide and water, performing activation reaction at 50-80° C. for 1-5 hours, and drying to obtain powder;

[0020] (2) In a protective atmosphere, the powder prepared in step (1) is heated to 800-1200° C. and carbonized for 1-5 hours to obtain a precursor material;

[0021] (3) Mix the precursor material with a soluble titanium salt and water, perform a hydrothermal reaction at 150-200° C. for 5-10 hours, wash, and dry to obtain the product.

[0022] As a preferred embodiment of the present invention, in step (1), the straw powder includes but is not limited to corn straw powder and wheat straw powder.

[0023] As a preferred embodiment of the present invention, in step (1), the soluble iron salt includes but is not limited to ferric chloride, ferric bromide, ferric sulfate, and ferric nitrate.

[0024] As a preferred embodiment of the present invention, in step (1), the soluble zinc salt includes but is not limited to zinc chloride, zinc bromide, zinc nitrate, and zinc sulfate.

[0025] As a preferred embodiment of the present invention, in step (1), the mass ratio of straw powder to ferric chloride, zinc chloride and potassium hydroxide is 10:0.5-1:0.5-1:0.5-1.5. The preferred mass ratio is 10:0.8:0.8:1.

[0026] As a preferred embodiment of the present invention, in step (1), the straw powder is prepared by drying, crushing and sieving the straw. The drying temperature is 150-200°C for 5-10 hours. The sieve mesh number is 200-400 mesh.

[0027] As a preferred embodiment of the present invention, in step (1), the activation reaction is carried out at 60° C. for 2 h.

[0028] As a preferred embodiment of the present invention, in step (1), the drying temperature is 60-100° C. and the drying time is 10-15 h.

[0029] As a preferred embodiment of the present invention, in step (2), the protective atmosphere uses nitrogen, argon or helium as the protective gas.

[0030] As a preferred embodiment of the present invention, in step (2), the heating rate is 5-15°C / min.

[0031] As a preferred embodiment of the present invention, in step (2), the carbonization treatment is carried out at 900° C. for 2 h, and the heating rate is 10° C. / min.

[0032] As a preferred embodiment of the present invention, in step (3), the soluble titanium salt includes but is not limited to titanium tetrachloride and titanium sulfate.

[0033] As a preferred embodiment of the present invention, in step (3), the ratio of the precursor material to titanium tetrachloride is 40-60 (mg): 5-10 (μL), preferably 50 (mg): 10 (μL).

[0034] As a preferred embodiment of the present invention, in step (3), the hydrothermal reaction is carried out at 180° C. for 8 h.

[0035] As a preferred embodiment of the present invention, in step (3), washing is performed with water and anhydrous ethanol for several times respectively.

[0036] The invention discloses an application of a biomass carbon-based material in preparing a zinc-air battery.

[0037] As a preferred embodiment of the present invention, in the zinc-air battery, biomass carbon-based material is used as the raw material for preparing the cathode.

[0038] A zinc-air battery, in which a biomass carbon-based material is used as a raw material for preparing a cathode.

[0039] As a preferred embodiment of the present invention, the anode of the zinc-air battery is metallic zinc.

[0040] As a preferred embodiment of the present invention, the electrolyte of the zinc-air battery is a potassium hydroxide solution.

[0041] Beneficial effects of the present invention:

[0042] The biomass carbon-based material provided by the present invention uses straw as the main raw material, adds soluble iron salt, soluble zinc salt, and potassium hydroxide to activate pores, and then calcined at high temperature to obtain a precursor material, and uses a soluble titanium salt as a reinforcing agent to modify the precursor material by a hydrothermal method to obtain a titanium-modified biomass carbon-based material, which has a more stable structure and catalytic performance and can be used as the positive electrode of a zinc-air battery. Among them, the main function of the soluble iron salt and the soluble zinc salt is to activate pores (zinc corrodes carbon, and iron ions are embedded in crystals after the carbon chain breaks), and potassium hydroxide is used for activation to increase the specific surface area and pore volume of the material and increase the channels for electron movement.

[0043] Studies have shown that zinc-air batteries based on titanium-modified biomass carbon-based materials have high power density and extremely high discharge stability, indicating that biomass carbon-based materials have good development prospects in the field of energy storage and conversion devices such as zinc-air batteries and fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 This is the XRD characterization diagram of the biomass carbon-based materials prepared in Experimental Examples 1 and 2.

[0045] Figure 2 SEM images of biomass carbon-based materials prepared in Experimental Examples 1 and 2.

[0046] Figure 3 LSV curves and power density curves of the biomass carbon-based material catalysts prepared in Examples 1 and 2 under specific test conditions.

[0047] Figure 4 This is the discharge curve of the zinc-air battery at different current densities in the experimental example.

[0048] Figure 5 The zinc-air battery in the experimental example is 10 mA / cm 2 Cycle diagram for charge and discharge cycles at current density .

[0049] In order to more clearly illustrate the technical solution to be protected by the present invention, the drawings in the embodiments or experimental examples are briefly introduced above. It should be understood that the above drawings should not be regarded as any limitation on the protection scope of the present invention. For ordinary technicians in this field, other related drawings can also be obtained based on these drawings without paying creative work. DETAILED DESCRIPTION

[0050] The technical solution of the present invention will be clearly and completely explained below in conjunction with specific embodiments and experimental examples.

[0051] Those skilled in the art should understand that the following embodiments and experimental examples are only used to illustrate the technical solutions and technical effects of the present invention and should not be regarded as any limitation on the protection scope of the present invention. Based on the following embodiments, other technical solutions obtained by those skilled in the art without creative work, such as technical solutions obtained after modification, deformation or simple replacement, all belong to the protection scope of the present invention.

[0052] Unless otherwise specified, the raw materials, reagents, and equipment used in the examples or experimental examples are all commercially available products.

[0053] Example 1

[0054] This embodiment provides a biomass carbon-based material, and the preparation method thereof comprises the following steps:

[0055] (1) The recovered wheat straw is placed in a drying oven at 180° C. and dried for 8 h to remove moisture, and the dried wheat straw is placed in a grinder and crushed and sieved to obtain a 300-mesh powder for later use;

[0056] (2) Using a micrometer balance, 10 g of the powder obtained in step (1) was weighed and placed in a three-necked flask, 1 g of potassium hydroxide, 0.8 g of zinc chloride and 0.8 g of ferric chloride were added, and then 10 mL of deionized water was added. The three-necked flask was placed in an oil bath at 60° C. and stirred for reaction for 2 h;

[0057] (3) After the reaction in step (2) is completed, the resulting viscous liquid is poured into a beaker, placed in a drying oven at 80° C. and dried for 12 h, and the resulting solid is placed in a mortar and ground into powder;

[0058] (4) placing the powder obtained in step (3) in a porcelain boat, placing it in a tube furnace for high-temperature calcination, setting the heating rate to 10°C / min, the carbonization temperature to 900°C, and carbonizing for 2h under nitrogen protection to obtain the precursor material W-900;

[0059] (5) Weigh 50 mg of the precursor material in step (4), add 5 μL of titanium tetrachloride and 31 mL of deionized water, stir at room temperature for 1.5 h, and then ultrasonicate to make it uniform. Place it in a reactor and perform hydrothermal reaction at 180 ° C for 8 h;

[0060] (6) After the reaction in step (5) is completed, the obtained product is washed three times with deionized water and once with anhydrous ethanol, the substrate is collected by centrifugation, and then dried and ground to obtain the biomass carbon-based material TiO2-W-900.

[0061] This embodiment also provides an application of a biomass carbon-based material in the preparation of a zinc-air battery.

[0062] This embodiment also provides a zinc-air battery, wherein biomass carbon-based material is used as a raw material for preparing the cathode.

[0063] In other embodiments and comparative examples of the present invention, the carbonization temperature in step (4) is set to 500°C, 700°C, 800°C, 1100°C, 1200°C to obtain biomass carbon-based materials. Experimental results show that 800-1200°C is a better temperature range, and 900°C is the best temperature.

[0064] Example 2

[0065] This embodiment provides a biomass carbon-based material, which differs from Embodiment 1 only in that corn straw is used instead of wheat straw. The rest is the same as Embodiment 1, and a precursor material C-900 and a biomass carbon-based material TiO2-C-900 are obtained.

[0066] This embodiment also provides an application of a biomass carbon-based material in the preparation of a zinc-air battery.

[0067] This embodiment also provides a zinc-air battery, wherein biomass carbon-based material is used as a raw material for preparing the cathode.

[0068] Example 3

[0069] This embodiment provides a biomass carbon-based material, and the preparation method thereof comprises the following steps:

[0070] (1) The recovered wheat straw is placed in a drying oven at 150° C. and dried for 10 h to remove moisture, and the dried wheat straw is placed in a grinder and crushed and sieved to obtain a 200-mesh powder for later use;

[0071] (2) Using a micrometer balance, 10 g of the powder obtained in step (1) was weighed and placed in a three-necked flask, 0.5 g of potassium hydroxide, 0.5 g of zinc chloride and 0.5 g of ferric chloride were added, and then 10 mL of deionized water was added. The three-necked flask was placed in an oil bath at 50° C. and stirred for 4 h;

[0072] (3) After the reaction in step (2) is completed, the resulting viscous liquid is poured into a beaker, placed in a drying oven at 60° C. and dried for 15 h, and the resulting solid is placed in a mortar and ground into powder;

[0073] (4) placing the powder obtained in step (3) in a porcelain boat, placing it in a tube furnace for high-temperature calcination, setting the heating rate to 5°C / min, the carbonization temperature to 800°C, and carbonizing for 4 hours under nitrogen protection to obtain a precursor material;

[0074] (5) Weigh 40 mg of the precursor material in step (4), add 5 μL of titanium tetrachloride and 31 mL of deionized water, stir at room temperature for 1.5 h, and then ultrasonicate to make it uniform. Place it in a reactor and perform hydrothermal reaction at 150° C. for 10 h.

[0075] (6) After the reaction in step (5) is completed, the obtained product is washed three times with deionized water and once with anhydrous ethanol, the substrate is collected by centrifugation, and then dried and ground to obtain a biomass carbon-based material.

[0076] This embodiment also provides an application of a biomass carbon-based material in the preparation of a zinc-air battery.

[0077] This embodiment also provides a zinc-air battery, wherein biomass carbon-based material is used as a raw material for preparing the cathode.

[0078] Example 4

[0079] This embodiment provides a biomass carbon-based material, and the preparation method thereof comprises the following steps:

[0080] (1) The recovered wheat straw is placed in a drying box at 200° C. and dried for 5 h to remove moisture, and the dried wheat straw is placed in a grinder and crushed and sieved to obtain a 400-mesh powder for later use;

[0081] (2) Using a micrometer balance, weigh 10 g of the powder obtained in step (1) and place it in a three-necked flask, add 1.5 g of potassium hydroxide, 1 g of zinc chloride and 1 g of ferric chloride, and then add 10 mL of deionized water, place the three-necked flask in an oil bath at 80° C. and stir to react for 1 h;

[0082] (3) After the reaction in step (2) is completed, the resulting viscous liquid is poured into a beaker, placed in a drying oven at 100° C. for 10 h, and the resulting solid is placed in a mortar and ground into powder;

[0083] (4) placing the powder obtained in step (3) in a porcelain boat, placing it in a tube furnace for high-temperature calcination, setting the heating rate to 15°C / min, the carbonization temperature to 1200°C, and carbonizing for 1 hour under nitrogen protection to obtain a precursor material;

[0084] (5) Weigh 60 mg of the precursor material in step (4), add 10 μL of titanium tetrachloride and 31 mL of deionized water, stir at room temperature for 1.5 h, and then ultrasonicate until uniform, place in a reactor, and perform hydrothermal reaction at 200 °C for 5 h;

[0085] (6) After the reaction in step (5) is completed, the obtained product is washed three times with deionized water and once with anhydrous ethanol, the substrate is collected by centrifugation, and then dried and ground to obtain a biomass carbon-based material.

[0086] This embodiment also provides an application of a biomass carbon-based material in the preparation of a zinc-air battery.

[0087] This embodiment also provides a zinc-air battery, wherein biomass carbon-based material is used as a raw material for preparing the cathode.

[0088] In other embodiments of the present invention, the soluble iron salt may be ferric bromide, ferric sulfate or ferric nitrate, the soluble zinc salt may be zinc bromide, zinc nitrate or zinc sulfate, and the soluble titanium salt may be titanium sulfate, which has almost no effect on the physicochemical properties and catalytic performance of the biomass carbon-based materials.

[0089] Experimental example

[0090] 1. XRD characterization

[0091] The biomass carbon-based material prepared in Example 2 was subjected to XRD characterization, and the results were as follows: Figure 1 shown.

[0092] from Figure 1 It can be seen that before coating, there is only the signal peak of KCl in the straw itself. The weak diffraction peak between 20°-26° is the characteristic peak of cellulose and hemicellulose in the straw. After coating, the signal peak of TiO2 can be seen.

[0093] 2. SEM analysis

[0094] The biomass carbon-based materials prepared in Examples 1 and 2 were analyzed by transmission electron microscopy. The results are as follows: Figure 2 shown.

[0095] from Figure 2 It can be seen that due to the porous tubular structure of straw, the biomass carbon-based material has a larger specific surface area and pore volume. This structure is conducive to the movement of electrons and can provide more channels for the movement of electrons. In addition, by comparing the electron microscope images before and after coating, it can be seen that TiO2 dotted on the surface of the material can increase the stability of the material.

[0096] 3. Electrochemical performance test

[0097] Weigh 10 mg of the biomass carbon-based material powder prepared in Examples 1 and 2, add it to 0.5 mL of the prepared mixed solution (the preparation ratio is: 370 μL of ionized water, 100 μL of isopropanol, 30 μL of Nation solution (5wt%, purchased from Sigma-Aldrich)), and disperse it ultrasonically to obtain a uniform and stable suspension; cut 2 cm × 5 cm nickel foam and 2 cm × 2 cm carbon black paper, use a tablet press to press the two together, absorb 100 μL of the suspension and evenly drip it on the carbon black paper, and after it is completely dried, use the zinc sheet as the anode, the nickel foam as the cathode, and the electrolyte using a saturated potassium hydroxide solution (6 mol / L) to assemble a simple zinc-air battery. Use an electrochemical workstation and blue electricity monitoring to test the electrochemical performance, and the obtained LSV curve is as follows: Figure 3 shown.

[0098] from Figure 3 It can be seen that biomass carbon-based material catalysts have excellent electrochemical properties.

[0099] Figure 4 For zinc-air batteries at 2 mA / cm 2 , 5mA / cm 2 , 10mA / cm 2 , 20mA / cm 2 , 50mA / cm 2 The discharge curves under five different current densities all showed a relatively stable state, further confirming its good stability.

[0100] Figure 5 The charge and discharge cycle stability test results, where the current density is 10mA / cm 2 , charging for 300s and discharging for 300s is one cycle, and the test obtains 100 cycle curves. The smooth curve shows that the biomass carbon-based material prepared in the embodiment has a great advantage in stability.

[0101] In the field of catalysts, biomass carbon-based materials have just come to the fore. However, traditional metal raw materials are expensive and difficult to mine, resulting in a small range of applications. Biomass carbon-based materials are simple and easy to obtain. From the perspective of agricultural products, they are waste utilization, killing two birds with one stone. They can recycle agricultural waste and ensure battery efficiency and stability. The material preparation process is relatively simple and the production cost is low.

[0102] Although the technical solution of the present invention has been described in detail above with general descriptions, specific implementation methods and experimental examples, it should be noted that the embodiments and experimental examples are only used to illustrate the technical solution and technical effects of the present invention, and should not be regarded as any limitation on the protection scope of the present invention. Simple deformation, modification or improvement based on the technical concept of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A biomass carbon-based material, characterized in that: The material uses straw as the main raw material, adds soluble iron salt, soluble zinc salt and potassium hydroxide to activate and form pores, and then calcines and carbonizes to obtain a precursor material, and then adds soluble titanium salt to heat to form a titanium dioxide surface modification layer to obtain a biomass carbon-based material.

2. The biomass carbon-based material according to claim 1, characterized in that: The straw includes but is not limited to corn straw and wheat straw; the soluble iron salt includes but is not limited to ferric chloride, ferric bromide, ferric sulfate, and ferric nitrate; the soluble zinc salt includes but is not limited to zinc chloride, zinc bromide, zinc nitrate, and zinc sulfate; the soluble titanium salt includes but is not limited to titanium tetrachloride and titanium sulfate.

3. The biomass carbon-based material according to claim 2, characterized in that: The activation pore making method comprises: mixing straw powder with ferric chloride, zinc chloride, potassium hydroxide and water, performing activation reaction at 50-80° C. for 1-5 hours, and drying to obtain powder.

4. The biomass carbon-based material according to claim 3, characterized in that: The calcination and carbonization process comprises heating the powder to 800-1200° C. in a protective atmosphere and performing carbonization treatment for 1-5 hours.

5. The biomass carbon-based material according to claim 2, characterized in that: The hydrothermal reaction is as follows: the precursor material is mixed with titanium tetrachloride and water, and the mixture is subjected to a hydrothermal reaction at 150-200° C. for 5-10 hours.

6. A method for preparing a biomass carbon-based material, characterized in that: The method comprises the following steps: (1) mixing straw powder with soluble iron salt, soluble zinc salt, potassium hydroxide and water, performing activation reaction at 50-80° C. for 1-5 hours, and drying to obtain powder; (2) In a protective atmosphere, the powder prepared in step (1) is heated to 800-1200° C. and carbonized for 1-5 hours to obtain a precursor material; (3) Mix the precursor material with a soluble titanium salt and water, perform a hydrothermal reaction at 150-200° C. for 5-10 hours, wash, and dry to obtain the product.

7. The preparation method according to claim 6, characterized in that: In step (1), the soluble iron salt includes but is not limited to ferric chloride, ferric bromide, ferric sulfate, and ferric nitrate; the soluble zinc salt includes but is not limited to zinc chloride, zinc bromide, zinc nitrate, and zinc sulfate; the mass ratio of straw powder to ferric chloride, zinc chloride, and potassium hydroxide is 10:0.5-1:0.5-1:0.5-1.

5.

8. The preparation method according to claim 6, characterized in that: In step (3), the soluble titanium salt includes but is not limited to titanium tetrachloride and titanium sulfate; the ratio of the precursor material to titanium tetrachloride is 40-60 (mg): 5-10 (μL).

9. Use of the biomass carbon-based material as described in any one of claims 1 to 5, or the biomass carbon-based material prepared by the method as described in any one of claims 6 to 8 in the preparation of a zinc-air battery.

10. A zinc-air battery, characterized in that: In the zinc-air battery, the biomass carbon-based material according to any one of claims 1 to 5, or the biomass carbon-based material prepared by the method according to any one of claims 6 to 8 is used as a raw material for preparing the cathode.

Citation Information

Patent Citations

  • Hollow spherical Fe and N co-doped porous carbon-based catalyst as well as preparation method and application thereof

    CN115224291A

  • Method for preparing loading functional oxide porous carbon

    CN101780952A

  • Biomass carbon catalyst and preparation method and application thereof

    CN105375042A

  • Preparation method of union modified activated carbon adsorbent for arsenic removal

    CN109277076A

  • Porous carbon, composite material, diaphragm modification material and application