Method for improving yield of high-purity silicon carbide raw material
By grinding and pretreating the carbon powder, changing its morphology, increasing the reaction activity, and improving the yield of silicon carbide raw materials, the problem of low solid phase synthesis yield is solved, and cost reduction and yield improvement are achieved.
Patent Information
- Application Number
- CN202411209386.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
AI Technical Summary
The yield of existing solid-phase synthetic silicon carbide raw materials is low, resulting in high raw material costs and it is difficult to meet the needs of reducing costs and increasing efficiency of silicon carbide crystals.
By grinding and pretreating the carbon powder, its morphology will change from flake-like to spherical shape, increasing the surface area and reactivity, and improving the yield of silicon carbide raw materials.
While maintaining the purity and particle size of the powder, the yield of silicon carbide raw materials will be increased by 15-30%. The process is simple and there is no need to add expensive equipment. It is suitable for mass production.
Abstract
Description
Technical Field
[0001] The invention relates to a method for improving the yield of high-purity silicon carbide raw materials, belonging to the technical field of third-generation semiconductor materials. Background Art
[0002] With the continuous development of technology, facing the higher performance requirements of the next generation of power electronic devices, the existing widely used semiconductor materials such as silicon (Si) and germanium (Ge) are increasingly unable to meet these new demands due to the limitations of their own physical and chemical properties. The discovery and development of the third generation of wide bandgap semiconductor materials represented by crystals such as silicon carbide (SiC) and gallium nitride (GaN) has brought new hope for the development of the next generation of power electronic devices.
[0003] Compared with traditional silicon materials, silicon carbide crystals have outstanding advantages such as wide band gap, high saturated electron mobility, high breakdown field strength, high thermal conductivity, etc., and their physical and chemical properties are also particularly stable. It is one of the best substrate materials for future power electronic devices. At present, power electronic devices made of silicon carbide materials have been widely used in important fields related to national economy and people's livelihood, such as transportation (electric vehicles, high-speed railways, rail transportation, aircraft, etc.), new energy, and communications.
[0004] After decades of development, the size and quality of silicon carbide crystals have become increasingly higher, and crystal growth and substrate processing technologies have become increasingly mature. However, the high price of silicon carbide substrates has severely restricted its wider application prospects. Therefore, reducing the cost of silicon carbide crystals is a common problem currently faced by the silicon carbide industry and is also a common goal for everyone to strive for.
[0005] In recent years, both the scientific research community and the industry have focused on reducing the cost of silicon carbide substrates by increasing the crystal diameter (8 inches), growing thicker crystals (thickness > 30 mm), developing new laser cutting technologies (reducing the loss and damage layer caused by multi-wire cutting), and developing new solution growth processes. However, the progress is not very obvious, and more new methods of reducing the cost and increasing the efficiency of silicon carbide crystals need to be considered from other angles.
[0006] High-purity silicon carbide raw materials are the core raw materials for the growth of high-quality silicon carbide crystals. Their purity, particle size and packing density will affect the yield and quality of silicon carbide crystals. Therefore, under the premise of ensuring high purity, coarse particle size and high packing density of raw materials, achieving the synthesis of low-cost silicon carbide raw materials is also one of the important contents and directions for reducing costs and increasing efficiency of silicon carbide crystals.
[0007] Patent 202310668650 discloses a device and method for preparing high-purity SiC polycrystalline rods. The method has high preparation efficiency, short growth cycle, single furnace output of more than 200 kg, silicon carbide purity of more than 99.99%, low input, high output, fundamentally reducing the cost of preparing SiC powder. Patent 202310384078 uses a specific isolation cylinder to grow silicon carbide single crystals using an isolation cylinder of a set size, effectively improving the temperature distribution inside the powder, reducing the axial temperature gradient and radial temperature gradient inside the powder, inhibiting the problem of silicon carbide powder crystallization in the center area of the crucible, and also reducing the crystallization phenomenon on the surface of the powder, thereby improving the utilization rate of silicon carbide powder. Patent 202310731030 discloses a method for preparing silicon carbide powder and silicon carbide powder. The mixed powder of silicon powder and carbon powder, silicon carbide powder and binder solution are mixed, and raw material microspheres are obtained by spray granulation. The obtained raw material microspheres are heat-treated to obtain silicon carbide powder. This method greatly shortens the preparation cycle of silicon carbide powder, thereby reducing production costs; at the same time, the silicon carbide powder prepared by the preparation method has a uniform particle size and large particles. The proportion of silicon carbide powder with a particle size of more than 0.5 mm can reach 80%, and the impurity content is low. Patent 202310391497 provides a method for recycling and reusing waste silicon carbide powder that cannot be used for crystal growth to produce silicon carbide powder. This solution opens up a new way for the reuse of waste silicon carbide powder and improves the utilization rate of waste silicon carbide powder. At the same time, it overcomes the problem of carbonization of silicon carbide powder synthesized in the prior art, which leads to a decrease in the final yield of silicon carbide, and improves the yield of silicon carbide powder synthesized from the carbon-silicon mixture.
[0008] The above patents respectively improve the yield of silicon carbide raw materials by means of synthesis device, optimization of internal temperature distribution of powder, spray granulation and waste recycling. However, the present invention has designed a simple and feasible new method to improve the yield of silicon carbide raw materials, which can increase the yield of existing raw materials by 15-30% while maintaining the purity and particle size of the powder unchanged, so as to meet the needs of reducing costs and increasing efficiency of silicon carbide crystals. Summary of the invention
[0009] In view of the problem that the existing solid-phase synthesis of silicon carbide raw materials has a low yield (less than 80%) and causes high raw material costs, the present invention pre-treats the carbon powder by grinding, so that the morphology of the carbon powder changes from scaly to spherical, increases the surface area of the carbon powder, improves the reaction activity, makes the raw material synthesis reaction more complete, and can increase the yield of silicon carbide raw materials by 15-30%; in addition, since grinding makes the morphology and particle size of the carbon powder more uniform, this also further improves the size uniformity of the synthetic raw materials. Compared with the existing process, only the grinding process is added, the process operation is convenient and simple, no expensive equipment is required, and batch production is possible. This method has significant advantages such as simple process and no reduction in the quality of raw materials, and provides a simple and easy method for mass production to improve the synthesis yield of silicon carbide raw materials.
[0010] The present invention discloses a method for improving the yield of silicon carbide raw materials, and the specific steps are as follows: (1) Pre-treating the carbon powder by grinding; (2) Using pre-treated carbon powder for batching; (3) Synthesis of silicon carbide raw materials; (4) Post-processing the raw materials to obtain silicon carbide raw materials.
[0011] The grinding in step (1) is generally mechanical grinding (including roller milling, roller grinding and ball milling, etc.) or air flow grinding, preferably ball milling and air flow milling; The pre-treatment of the carbon powder by grinding in step (1) means that the morphology of the carbon powder changes from a scaly shape before treatment to a spherical shape after treatment after grinding; The grinding is preferably ball milling and air flow milling, wherein the ball milling can be cylindrical ball milling, conical ball milling, tube milling or planetary ball milling, etc., preferably cylindrical ball milling; In the cylindrical ball mill, the total volume of silicon carbide microspheres and carbon material added to the grinding jar should not exceed 80% of the volume of the grinding jar, preferably 40-60%; The weight ratio of the silicon carbide balls to the carbon powder added to the grinding tank is 1:3 to 1:7, preferably 1:5; The parameters of the ball mill or jet mill can be selected based on the comprehensive selection of the equipment, with the change of the carbon powder morphology from flaky to spherical as the judgment standard; The batching as described in step (2) refers to weighing silicon powder and pre-treated carbon powder according to a set formula and mixing the two uniformly; The synthesis of silicon carbide raw materials as described in step (3) refers to the use of any method to chemically react silicon powder and carbon powder to grow silicon carbide powder, which can be an Acheson method, a CVD method or a solid phase synthesis method, wherein the solid phase synthesis method is preferred; The post-processing of raw materials as described in step (4) refers to processing the synthesized raw materials in any manner to make them capable of growing silicon carbide crystals.
[0012] Compared with the prior art, the present invention has the following beneficial effects: 1. By grinding and regulating the morphology of carbon powder, the surface area of carbon powder is increased, the reaction activity is improved, the synthesis reaction is more complete, and the yield of silicon carbide raw materials is increased (increased by 15-30%); 2. Improve the morphological consistency of carbon powder and make the synthesized raw materials more uniform; 3. Compared with the existing process, only the grinding process is added, the process is convenient and simple to operate, no expensive equipment is required, and batch production is possible; 4. It does not affect the purity, particle size and bulk density of the raw materials, and can meet the powder requirements of silicon carbide crystal growth. DETAILED DESCRIPTION
[0013] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0014] The present invention provides a technical solution: Example
[0015] (1) The carbon powder was pretreated by grinding. The carbon powder and silicon carbide balls made of high-purity silicon carbide material (5N) were placed in a plastic ball mill at a weight ratio of 5:1, accounting for about 60% of the total volume. The ball mill was placed on a cylindrical ball mill and ball milled at 50 rpm for 1 h. After ball milling, the carbon powder had a spherical morphology. (2) Weighing the pretreated carbon powder and silicon powder according to the chemical equation and loading them into a mixer for mixing; (3) The mixed material from the previous step is loaded into a synthesis furnace and the raw material is synthesized by a solid phase synthesis method; (4) The synthesized raw materials are taken out and post-processed such as screening, cleaning, drying and packaging to obtain silicon carbide raw materials. The yield of the raw materials is 85%. Example
[0016] (1) Pre-treating the carbon powder by grinding, adding the carbon powder into a jet mill, using inert gas as the gas, and adjusting the feed speed so that the carbon powder after grinding is spherical; (2) Weighing the pretreated carbon powder and silicon powder according to the chemical equation and loading them into a mixer for mixing; (3) The mixed material from the previous step is loaded into a synthesis furnace and the raw material is synthesized by a solid phase synthesis method; (4) The synthesized raw materials are taken out and post-processed such as screening, cleaning, drying and packaging to obtain silicon carbide raw materials. The yield of the raw materials is 86%. Comparative Example 1 (1) Directly use commercially available carbon powder (without ball milling); (2) Weighing the pretreated carbon powder and silicon powder according to the chemical equation and loading them into a mixer for mixing; (3) The mixed material from the previous step is loaded into a synthesis furnace and the raw material is synthesized by a solid phase synthesis method; (4) The synthesized raw materials are taken out and post-processed such as screening, cleaning, drying and packaging to obtain silicon carbide raw materials. The yield of the raw materials is 66%. Example
[0017] (1) The carbon powder was pretreated by grinding. The carbon powder and silicon carbide balls made of high-purity silicon carbide material (5N) were placed in a plastic ball mill at a weight ratio of 5:1, accounting for about 60% of the total volume. The ball mill was placed on a cylindrical ball mill and ball milled at 50 rpm for 1 h. After ball milling, the carbon powder had a spherical morphology. (2) Silicon powder and carbon powder are weighed according to a molar ratio of 1.01:1, and the silicon powder and the pretreated carbon powder are loaded into a mixer for mixing; (3) The mixed material from the previous step is loaded into a synthesis furnace and the raw material is synthesized by a solid phase synthesis method; (4) The synthesized raw materials are taken out and post-processed such as screening, cleaning, drying and packaging to obtain silicon carbide raw materials. The yield of the raw materials is 89%. Example
[0018] (1) Pre-treating the carbon powder by grinding, adding the carbon powder into a jet mill, using inert gas as the gas, and adjusting the feed speed so that the carbon powder after grinding is spherical; (2) Silicon powder and carbon powder are weighed according to a molar ratio of 1.01:1, and the silicon powder and the pretreated carbon powder are loaded into a mixer for mixing; (3) The mixed material from the previous step is loaded into a synthesis furnace and the raw material is synthesized by a solid phase synthesis method; (4) The synthesized raw materials are taken out and post-processed such as screening, cleaning, drying and packaging to obtain silicon carbide raw materials. The yield of the raw materials is 91%. Comparative Example 2 (1) Directly use commercially available carbon powder (without ball milling); (2) Silicon powder and carbon powder are weighed according to a molar ratio of 1.01:1, and the silicon powder and the pretreated carbon powder are loaded into a mixer for mixing; (3) The mixed material from the previous step is loaded into a synthesis furnace and the raw material is synthesized by a solid phase synthesis method; (4) The synthesized raw materials are taken out and post-processed such as screening, cleaning, drying and packaging to obtain silicon carbide raw materials. The yield of the raw materials is 65%. Example
[0019] (1) The carbon powder was pretreated by grinding. The carbon powder and silicon carbide balls made of high-purity silicon carbide material (5N) were loaded into a plastic ball mill at a weight ratio of 3:1, accounting for about 60% of the total volume. The ball mill was installed on a cylindrical ball mill and ball milled at a speed of 50 rpm for 1 h. After ball milling, the carbon powder had a spherical morphology. (2) Weighing the pretreated carbon powder and silicon powder according to the chemical equation and loading them into a mixer for mixing; (3) The mixed material from the previous step is loaded into a synthesis furnace and the raw material is synthesized by a solid phase synthesis method; (4) The synthesized raw materials are taken out and post-processed such as screening, cleaning, drying and packaging to obtain silicon carbide raw materials. The yield of the raw materials is 81%. Example
[0020] (1) The carbon powder was pretreated by grinding. The carbon powder and silicon carbide balls made of high-purity silicon carbide material (5N) were loaded into a plastic ball mill at a weight ratio of 7:1, accounting for about 60% of the total volume. The ball mill was installed on a cylindrical ball mill and ball milled at a speed of 50 rpm for 1 h. After ball milling, the carbon powder had a spherical morphology. (2) Weighing the pretreated carbon powder and silicon powder according to the chemical equation and loading them into a mixer for mixing; (3) The mixed material from the previous step is loaded into a synthesis furnace and the raw material is synthesized by a solid phase synthesis method; (4) The synthesized raw materials are taken out and post-processed such as screening, cleaning, drying and packaging to obtain silicon carbide raw materials. The yield of the raw materials is 83%. Example
[0021] (1) The carbon powder was pretreated by grinding. The carbon powder and silicon carbide balls made of high-purity silicon carbide material (5N) were loaded into a plastic ball mill at a weight ratio of 3:1, accounting for about 60% of the total volume. The ball mill was installed on a cylindrical ball mill and ball milled at 30 rpm for 0.5 h. After ball milling, the carbon powder had a spherical morphology. (2) Weighing the pretreated carbon powder and silicon powder according to the chemical equation and loading them into a mixer for mixing; (3) The mixed material from the previous step is loaded into a synthesis furnace and the raw material is synthesized by a solid phase synthesis method; (4) The synthesized raw materials are taken out and post-processed such as screening, cleaning, drying and packaging to obtain silicon carbide raw materials. The yield of the raw materials is 76%. Example
[0022] (1) The carbon powder was pretreated by grinding. The carbon powder and silicon carbide balls made of high-purity silicon carbide material (5N) were loaded into a plastic ball mill at a weight ratio of 3:1, accounting for about 60% of the total volume. The ball mill was installed on a cylindrical ball mill and ball milled at 50 rpm for 2 h. After ball milling, the carbon powder had a spherical morphology. (2) Weighing the pretreated carbon powder and silicon powder according to the chemical equation and loading them into a mixer for mixing; (3) The mixed material from the previous step is loaded into a synthesis furnace and the raw material is synthesized by a solid phase synthesis method; (4) The synthesized raw materials are taken out and post-processed such as screening, cleaning, drying and packaging to obtain silicon carbide raw materials. The yield of the raw materials is 84%. Comparative Example 3 (1) The carbon powder was pretreated by grinding. The carbon powder and silicon carbide balls made of high-purity silicon carbide material (5N) were loaded into a plastic ball mill at a weight ratio of 10:1, accounting for about 60% of the total volume. The ball mill was installed on a cylindrical ball mill and ball milled at a speed of 30 rpm for 0.5 h. After ball milling, the carbon powder had a spherical morphology. (2) Weighing the pretreated carbon powder and silicon powder according to the chemical equation and loading them into a mixer for mixing; (3) The mixed material from the previous step is loaded into a synthesis furnace and the raw material is synthesized by a solid phase synthesis method; (4) The synthesized raw materials are taken out and post-processed such as screening, cleaning, drying and packaging to obtain silicon carbide raw materials. The yield of the raw materials is 66%.
[0023] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for improving the yield of high-purity silicon carbide raw materials, characterized in that: Specific steps as follows: (1) Pre-treating the carbon powder by grinding; (2) Using pre-treated carbon powder for batching; (3) Synthesis of silicon carbide raw materials; (4) Post-processing the raw materials to obtain silicon carbide raw materials; The grinding in step (1) is generally mechanical pulverization or air flow pulverization, preferably ball milling and air flow milling; The pre-treatment of the carbon powder by grinding in step (1) means that the morphology of the carbon powder changes from a scaly shape before treatment to a spherical shape after treatment after grinding; The grinding is preferably ball milling and air flow milling, wherein the ball milling can be cylindrical ball milling, conical ball milling, tube milling or planetary ball milling, etc., preferably cylindrical ball milling; In the cylindrical ball mill, the total volume of silicon carbide microspheres and carbon material added to the grinding jar should not exceed 80% of the volume of the grinding jar, preferably 40-60%; The weight ratio of the silicon carbide balls to the carbon powder added to the grinding tank is 1:3 to 1:7, preferably 1:5; The parameters of the ball mill or jet mill can be selected based on the comprehensive selection of the equipment, with the change of the carbon powder morphology from flaky to spherical as the judgment standard; The batching described in step (2) refers to weighing silicon powder and pre-treated carbon powder according to a set formula and mixing the two uniformly; (3) The synthesis of silicon carbide raw materials in step (3) refers to the use of any method to chemically react silicon powder and carbon powder to grow silicon carbide powder, which can be Acheson method, CVD method or solid phase synthesis method, among which solid phase synthesis method is preferred; The post-processing of raw materials in step (4) refers to processing the synthesized raw materials in any manner to make them capable of growing silicon carbide crystals.