Method for preparing silicon dioxide microspheres from waste glass fiber reinforced plastics and application of silicon dioxide microspheres

The glass fibers were recovered through the pyrolysis-oxidation method and high-performance silica microspheres were prepared, which solved the problem of low resource value of waste fiberglass, and achieved efficient resource reuse and catalytic performance improvement.

CN118929675APending Publication Date: 2024-11-12GUODIAN SCI & TECH RES INST +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410975148.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the reuse and resource utilization value of glass fiber fiber recycling from waste fiber reinforced fiberglass materials is low and it is difficult to convert it into high-value products.

Method used

Glass fibers were recovered by pyrolysis-oxidation method, and silica microspheres with high specific surface area and controllable pore structure were prepared by polymerization-induced colloid aggregation method, used as catalyst support, and the catalyst was constructed by supporting Cu.

Benefits of technology

The resource value of waste fiberglass has been improved. The prepared silica microspheres have good catalytic properties, the hydrogenation conversion rate of furfural can reach 94.7%, and the selectivity of furfurfural alcohol can reach 96.9%, making the process simple and efficient.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929675A_ABST
    Figure CN118929675A_ABST
Patent Text Reader

Abstract

The invention relates to the field of solid waste recycling, and discloses a method for preparing silicon dioxide microspheres from waste glass fiber reinforced plastics and application. The method comprises the following steps: recycling glass fiber from a waste glass fiber reinforced plastic material in the retired fan blade through pyrolysis and oxidation treatment, preparing silicon dioxide sol by taking the glass fiber as a silicon source, and preparing the silicon dioxide microspheres from the obtained silicon dioxide sol through a polymerization-induced colloid aggregation method. The silicon dioxide microspheres prepared by the method have a large specific surface area and a controllable pore structure, and are beneficial to loading and exposing more active sites when being used as a catalyst carrier, so that the performance of a catalyst is improved. The invention provides a new waste glass fiber reinforced plastic resource reutilization process, the glass fiber component is effectively recycled, the resource value is improved, and the application prospect is wide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of solid waste resource utilization, and in particular to a method for preparing silicon dioxide microspheres by utilizing waste glass fiber reinforced plastics and an application thereof. Background Art

[0002] Wind power generation is a green energy industry that has received widespread attention in recent years. The wind turbine blades used for power generation are mainly made of glass fiber reinforced materials (i.e., FRP) based on organic resins, and their service life is generally 15-20 years. With the popularization and promotion of wind power generation, a large amount of waste FRP will be generated after the wind turbine blades reach the end of their service life. Traditional landfill and incineration treatments are not only inefficient, but also cause resource waste and environmental pollution. Therefore, it is urgent to develop corresponding resource recycling routes to improve economic value. Among the FRP materials used in wind turbine blades, the mass proportion of glass fiber can generally reach 60-70wt%, and the cost accounts for the highest proportion, with the highest recycling value. How to efficiently recycle the glass fiber in retired wind turbine blades is one of the research hotspots.

[0003] At present, pyrolysis is one of the methods for recycling glass fibers in FRP materials of retired wind turbine blades. However, the recycled glass fibers obtained by pyrolysis have defects such as short size and reduced mechanical properties, and there is no suitable utilization channel for the time being. It is difficult to use them directly as glass fibers, and the resource value is low. Therefore, it is necessary to develop a process route that can effectively recycle glass fibers in retired wind turbine blades and transform them into new high-value products to improve the resource value of retired wind turbine blades. Summary of the invention

[0004] The purpose of the present invention is to overcome the problem of low recycling value of glass fiber recycled from waste FRP materials in the prior art, and provide a method and application of preparing silica microspheres using waste FRP. The method recycles glass fiber from waste FRP materials of retired wind turbine blades by pyrolysis-oxidation method, then prepares silica sol with the recycled glass fiber, and further prepares silica microspheres by polymerization-induced colloidal aggregation method, and the process is effective and controllable; the silica microspheres prepared by the method have a high specific surface area and controllable pore structure, and contain metal elements such as Cu, Al, and Mg, and can be used as a catalyst carrier. The catalyst is constructed by further loading Cu, and exhibits good furfural hydrogenation performance.

[0005] In order to achieve the above object, the present invention provides a method for preparing silica microspheres using waste glass fiber reinforced plastics, comprising the following steps: (1) crushing the waste FRP, performing pyrolysis and oxidation treatments, and recovering the glass fibers; (2) grinding the glass fiber into a glass fiber powder of 100-300 mesh, mixing it with a first alkali, performing a first calcination treatment, mixing the calcined product with water, performing solid-liquid separation, and then mixing the liquid obtained by the solid-liquid separation with a first acid to obtain a silica sol; (3) mixing the silica sol with a urea solution, adjusting the pH to ≤ 4 with a second acid, and then mixing with a formaldehyde solution and reacting; (4) A second base is added to the mixture obtained in the reaction of step (3) to adjust the pH value to 2-10, and then the mixture is mixed with a hexadecyltrimethylammonium bromide solution and allowed to stand, and the mixture obtained after standing is subjected to solid-liquid separation, and then the obtained solid is dried and subjected to a second calcination treatment.

[0006] Preferably, the waste fiberglass comes from retired wind turbine blades.

[0007] Preferably, in step (1), the pyrolysis treatment is carried out in an inert atmosphere, and the conditions of the pyrolysis treatment include: a temperature of 400-700° C. and a time of 10-60 min.

[0008] Preferably, the inert atmosphere is a nitrogen atmosphere and / or an argon atmosphere.

[0009] Preferably, in step (1), the oxidation treatment is carried out in an oxygen-containing atmosphere, and the conditions of the oxidation treatment include: a temperature of 400-700° C. and a time of 10-60 min.

[0010] Preferably, the oxygen-containing atmosphere is an air atmosphere and / or an oxygen atmosphere.

[0011] Preferably, in step (2), the mass ratio of the glass fiber powder to the first alkali is 1:0.5-2.

[0012] Preferably, in step (2), the first calcination treatment is carried out in an inert atmosphere, and the conditions of the first calcination treatment include: a temperature of 450-750° C. and a time of 1-6 hours.

[0013] Preferably, the inert atmosphere is a nitrogen atmosphere and / or an argon atmosphere.

[0014] Preferably, in step (3), the volume ratio of the silica sol to the urea solution is 1:1-3.

[0015] Preferably, the concentration of the urea solution is 60-100 g / L.

[0016] Preferably, the volume ratio of the silica sol to the formaldehyde solution is 1.5-3:1; Preferably, the concentration of the formaldehyde solution is 25-45wt%.

[0017] Preferably, in step (3), the reaction conditions include: stirring at 600-1000 rpm for 1-5 min, and then standing for 8-24 h.

[0018] Preferably, in step (4), the conditions of the second calcination treatment include: a temperature of 500-700° C. and a time of 0.5-3 h.

[0019] Preferably, in step (4), the volume ratio of the silica sol to the hexadecyltrimethylammonium bromide solution is 1:1.5-3.5; Preferably, the concentration of the hexadecyltrimethylammonium bromide solution is 6-10 g / L.

[0020] Preferably, the first base and the second base are the same or different, and each is at least one of sodium hydroxide, potassium hydroxide and sodium carbonate.

[0021] Preferably, the first acid and the second acid are the same or different, and each is at least one of dilute sulfuric acid, dilute hydrochloric acid and glacial acetic acid.

[0022] The second aspect of the present invention provides silica microspheres prepared by the above method.

[0023] The third aspect of the present invention provides the use of the aforementioned silica microspheres as catalyst carriers.

[0024] According to the preparation method of silica microspheres of the present invention, glass fibers can be recovered from waste fiberglass materials of retired wind turbine blades by a pyrolysis-oxidation method, and the glass fibers can be converted into silica sols. Then, silica microspheres with a large specific surface area and adjustable structure are prepared by a polymerization-induced colloidal aggregation method. A new waste fiberglass resource recovery process is provided, and recycled products with higher added value are obtained, thereby improving the resource recovery value. The overall process is simple and efficient, and has good application prospects.

[0025] The silica microspheres prepared according to the preparation method of the present invention can control the structural characteristics of the silica microspheres by adjusting the conditions of the preparation process to meet different needs; the silica microspheres have a large specific surface area, and when used as a catalyst carrier, they have more active sites, which is conducive to obtaining better catalytic performance, and when the waste fiberglass material of retired wind turbine blades is used as a raw material, it also contains metal elements such as Cu, Mg and Al, which further improves the catalytic performance; the catalyst using the silica microspheres as a carrier to load Cu shows good performance in catalyzing the hydrogenation of furfural to prepare furfuryl alcohol, and the furfural conversion rate can reach 94.7%, and the furfuryl alcohol selectivity can reach 96.9%. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The present invention provides a schematic flow chart of a method for preparing silicon dioxide microspheres by using waste glass fiber reinforced plastics. DETAILED DESCRIPTION

[0027] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0028] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0029] The present invention provides a method for preparing silicon dioxide microspheres by using waste glass fiber reinforced plastics, comprising the following steps: (1) crushing the waste FRP, performing pyrolysis and oxidation treatments, and recovering the glass fibers; (2) grinding the glass fiber into a glass fiber powder of 100-300 mesh, mixing it with a first alkali, performing a first calcination treatment, mixing the calcined product with water, performing solid-liquid separation, and then mixing the liquid obtained by the solid-liquid separation with a first acid to obtain a silica sol; (3) mixing the silica sol with a urea solution, adjusting the pH to ≤ 4 with a second acid, and then mixing with a formaldehyde solution and reacting; (4) A second base is added to the mixture obtained in the reaction of step (3) to adjust the pH value to 2-10, and then the mixture is mixed with a hexadecyltrimethylammonium bromide solution and allowed to stand, and the mixture obtained after standing is subjected to solid-liquid separation, and then the obtained solid is dried and subjected to a second calcination treatment.

[0030] In the method of the present invention, preferably, the waste FRP comes from retired fan blades. In the present invention, retired fan blades are used as the source of waste FRP, and the prepared silica microspheres also contain other metal components such as Cu, Al, Mg, etc., which is beneficial to further improve the activity of the catalyst when used as a catalyst carrier.

[0031] In the method of the present invention, preferably, in step (1), the pyrolysis treatment is carried out in an inert atmosphere, and the conditions of the pyrolysis treatment include: a temperature of 400-700°C and a time of 10-60 min. More preferably, the conditions of the pyrolysis treatment include: in an inert atmosphere, a temperature of 425-600°C and a time of 15-50 min. Most preferably, the conditions of the pyrolysis treatment include: in an inert atmosphere, a temperature of 450-550°C and a time of 20-40 min. In the present invention, the above-mentioned pyrolysis conditions can be used to fully decompose the resin component in the waste fiberglass material of the waste fan blades, leaving the glass fiber component containing residual carbon, which is conducive to subsequent processing to obtain pure glass fiber.

[0032] In the method of the present invention, preferably, the inert atmosphere is a nitrogen atmosphere and / or an argon atmosphere.

[0033] In the method of the present invention, preferably, in step (1), the oxidation treatment is carried out in an oxygen-containing atmosphere, and the conditions of the oxidation treatment include: a temperature of 400-700°C and a time of 10-60 min. More preferably, the conditions of the oxidation treatment include: carried out in an oxygen-containing atmosphere, a temperature of 425-600°C, and a time of 15-50 min. Most preferably, the conditions of the oxidation treatment include: carried out in an oxygen-containing atmosphere, a temperature of 450-550°C, and a time of 20-40 min. In the present invention, by adopting the above-mentioned oxidation conditions, the residual carbon in the glass fiber component containing residual carbon obtained in the aforementioned pyrolysis step can be fully oxidized, thereby recovering pure glass fibers.

[0034] In the method of the present invention, preferably, the oxygen-containing atmosphere is an air atmosphere and / or an oxygen atmosphere.

[0035] In the method of the present invention, preferably, in step (2), the mass ratio of the glass fiber powder to the first alkali is 1:0.5-2, more preferably 1:0.5-1.5, and most preferably 1:0.75-1.25. In the present invention, the above-mentioned amount of the first alkali can provide enough alkali to convert the glass fiber, which is conducive to increasing the recovery of the glass fiber.

[0036] In the method of the present invention, preferably, in step (2), the first calcination treatment is carried out under an inert atmosphere, and the conditions of the first calcination treatment include: a temperature of 450-750°C and a time of 1-6h. More preferably, the conditions of the first calcination treatment include: a temperature of 500-700°C and a time of 1.5-4.5h. Most preferably, the conditions of the first calcination treatment include: a temperature of 550-650°C and a time of 2-3h. In the present invention, the above-mentioned conditions of the first calcination treatment can make the glass fiber and the first alkali react fully to generate a soluble component, which is beneficial to the subsequent treatment to generate a silica sol.

[0037] In the method of the present invention, preferably, the inert atmosphere is a nitrogen atmosphere and / or an argon atmosphere.

[0038] In the method of the present invention, preferably, in step (3), the volume ratio of the silica sol to the urea solution is 1:1-3, more preferably 1:1.2-2, and most preferably 1:1.25-1.75.

[0039] In the method of the present invention, preferably, the concentration of the urea solution is 60-100 g / L, more preferably 70-90 g / L, most preferably 75-85 g / L.

[0040] In the method of the present invention, preferably, the volume ratio of the silica sol to the formaldehyde solution is 1.5-3:1, more preferably 1.5-2.5:1, and most preferably 1.75-2.25:1.

[0041] In the method of the present invention, preferably, the concentration of the formaldehyde solution is 25-45wt%, more preferably 30-40wt%, most preferably 32-37wt%.

[0042] In the present invention, the above-mentioned amounts of urea and formaldehyde solution are used to undergo a polymerization reaction to generate an appropriate amount of urea-formaldehyde resin, which together with the silica sol forms urea-formaldehyde resin / SiO2 composite microspheres, which is beneficial for the silica microspheres obtained after subsequent treatment to maintain their shape without breaking or collapsing.

[0043] In the method of the present invention, preferably, in step (3), the reaction conditions include: stirring at 600-1000 rpm for 1-5 min, and then standing for 8-24 h. More preferably, the reaction conditions include: stirring at 700-900 rpm for 1-4 min, and then standing for 10-20 h. Most preferably, the reaction conditions include: stirring at 750-850 rpm for 1-3 min, and then standing for 10-15 h. In the present invention, the above reaction conditions can be used to initiate a polymerization reaction to generate urea-formaldehyde resin and form urea-formaldehyde resin / SiO2 composite microspheres together with silica sol.

[0044] In the method of the present invention, preferably, in step (4), the conditions of the second calcination treatment include: a temperature of 500-700°C and a time of 0.5-3h. More preferably, the conditions of the second calcination treatment include: a temperature of 525-675°C and a time of 0.5-2h. Most preferably, the conditions of the second calcination treatment include: a temperature of 550-650°C and a time of 0.75-1.5h. In the present invention, the above-mentioned conditions of the second calcination treatment can fully pyrolyze and volatilize the urea-formaldehyde resin in the aforementioned urea-formaldehyde resin / SiO2 composite microspheres, leaving the silica component to form silica microspheres.

[0045] In the method of the present invention, preferably, in step (4), the volume ratio of the silica sol to the hexadecyltrimethylammonium bromide solution is 1:1.5-3.5, more preferably 1:1.5-2.5, and most preferably 1:1.75-2.25.

[0046] In the method of the present invention, preferably, in step (4), the concentration of the hexadecyltrimethylammonium bromide solution is 6-10 g / L, more preferably 7-9 g / L, and most preferably 7.5-8.5 g / L.

[0047] In the method of the present invention, preferably, in step (4), the silica sol and the hexadecyltrimethylammonium bromide solution are mixed and allowed to stand for 3-10 hours, more preferably 4-9 hours, and most preferably 5-8 hours.

[0048] In the method of the present invention, preferably, the first alkali and the second alkali are the same or different, and each is at least one of sodium hydroxide, potassium hydroxide and sodium carbonate. More preferably, the first alkali and the second alkali are sodium hydroxide.

[0049] In the method of the present invention, preferably, the first acid and the second acid are the same or different, and each is at least one of dilute sulfuric acid, dilute hydrochloric acid and glacial acetic acid. More preferably, the first acid and the second acid are glacial acetic acid.

[0050] In a specific embodiment, Figure 1 As shown, the method for preparing silica microspheres using waste glass fiber reinforced plastics of the present invention comprises the following steps: (1) Waste FRP from retired wind turbine blades is crushed and pyrolyzed in an inert atmosphere at 400-700°C for 10-60 min, and then oxidized in an oxygen-containing atmosphere at 400-700°C for 10-60 min to obtain glass fibers; (2) grinding the glass fiber into a glass fiber powder of 100-300 mesh, mixing the glass fiber powder with the first alkali in a mass ratio of 1:0.5-2, and then performing a first calcination treatment in a polysulfate atmosphere at 450-750° C. for 1-6 hours; then mixing the obtained calcined product with water, stirring for 8-16 hours, and then performing solid-liquid separation, and then mixing the liquid obtained by the solid-liquid separation with the first acid to obtain a silica sol; (3) mixing the silica sol with 60-100 g / L urea solution in a volume ratio of 1:1-3, adjusting the pH to ≤ 4 with a second acid, and then mixing with 25-45 wt % formaldehyde solution in a volume ratio of 1.5-3:1, then stirring at 600-1000 rpm for 1-5 min, and then standing to react for 8-24 h; (4) adding a second base to the mixture obtained in step (3) to adjust the pH value to 2-10, and then mixing it with 6-10 g / L of hexadecyltrimethylammonium bromide solution in a volume ratio of 1:1.5-3.5 of the silica sol to the hexadecyltrimethylammonium bromide solution, stirring for 10-30 min and then standing for 3-10 h, separating the obtained mixture from solid and liquid, and drying the obtained solid at 90-120° C. for 6-18 h, and then performing a second calcination treatment at 500-700° C. for 0.5-3 h; The first base and the second base are the same or different, and each is at least one of sodium hydroxide, potassium hydroxide and sodium carbonate; the first acid and the second acid are the same or different, and each is at least one of dilute sulfuric acid, dilute hydrochloric acid and glacial acetic acid.

[0051] According to the method for preparing silica microspheres using waste FRPs described in the present invention, glass fibers are first recovered from waste FRP materials of retired wind turbine blades by a pyrolysis-oxidation method, and the glass fibers are converted into silica sols. Then, silica microspheres with a large specific surface area and adjustable structure are prepared by a polymerization-induced colloidal aggregation method. This provides a new waste FRP resource recovery process, effectively recovers and utilizes glass fibers in waste FRPs, improves the resource recovery value, and the overall process is efficient and controllable, with good application prospects.

[0052] The present invention also provides silica microspheres prepared by the above method, wherein the silica microspheres can control the structural characteristics of the final product by adjusting the conditions of the preparation process to adapt to different application requirements; the silica microspheres have a large specific surface area of ​​up to 658 m 2 / g, so when used as a catalyst carrier, it has more active sites, which is conducive to obtaining better catalytic performance; and because it is made of waste FRP (especially waste FRP from retired wind turbine blades), it also contains metal elements such as Cu, Mg and Al, which further improves the catalytic performance.

[0053] The present invention also provides the use of the aforementioned silica microspheres as catalyst carriers, specifically including using the silica microspheres as carriers to load active components to prepare corresponding catalysts.

[0054] In the application of the present invention, preferably, the silica microspheres are used as a carrier of a Cu-containing catalyst. In the present invention, since the silica microspheres contain metal elements such as Cu, when used as a Cu-containing catalyst carrier, the content of Cu active components can be further increased, which is conducive to further improving the catalytic performance.

[0055] In the application of the present invention, preferably, the following steps are included: using the silica microspheres as a carrier, loading Cu by an equal volume impregnation method, and obtaining a Cu / SiO2 catalyst.

[0056] In a specific embodiment, the use of the aforementioned silica microspheres of the present invention as catalyst carriers includes: mixing the silica microspheres of the present invention with an aqueous solution of a copper salt (such as copper nitrate) according to an equal volume impregnation method, drying the obtained suspension, and then calcining the solid obtained after drying in an oxygen-containing atmosphere (such as an air atmosphere) (for example, at a temperature of 450-550°C), and then calcining again in a reducing atmosphere (such as a hydrogen atmosphere) (for example, at a temperature of 380-420°C) to obtain a Cu / SiO2 catalyst loaded with Cu.

[0057] The catalyst further loaded with Cu was prepared by using the silica microspheres as a carrier, which showed good performance in catalyzing the hydrogenation of furfural to produce furfuryl alcohol, with a furfural conversion rate of up to 94.7% and a furfuryl alcohol selectivity of up to 96.9%.

[0058] The following examples further illustrate the method for preparing silica microspheres using waste glass fiber reinforced plastics and its application. The examples are implemented based on the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following examples.

[0059] The experimental methods in the following examples, unless otherwise specified, are all conventional methods in the art. The experimental materials used in the following examples, unless otherwise specified, are all commercially available.

[0060] Example 1 (1) 50 g of retired fan blades were crushed and placed in a fixed bed reactor, and pyrolyzed in a nitrogen atmosphere at 500° C. for 30 min to completely decompose the organic resin component to obtain glass fibers containing residual carbon; then the glass fibers containing residual carbon were oxidized in an air atmosphere at 500° C. for 30 min to completely remove the residual carbon to obtain glass fibers; (2) Grinding the glass fiber obtained in step (1) into a 200-mesh glass fiber powder, mixing 20 g of the glass fiber powder with 20 g of sodium hydroxide, and then calcining at 600° C. for 2 h; grinding the calcined product and mixing it with 200 mL of deionized water, and then magnetically stirring it for 12 h to obtain a suspension; filtering the obtained suspension, and dripping glacial acetic acid into the liquid obtained by filtration until gelation occurs, thereby obtaining a silica sol; (3) 100 mL of the silica sol obtained in step (2) was mixed with 150 mL of urea solution (concentration of 80 g / L) and stirred evenly, and the pH value was adjusted to 2 with glacial acetic acid, and then 50 mL of formaldehyde solution (concentration of 35 wt%) was quickly added to the pH-adjusted mixture, stirred at a rate of 800 rpm for 2 min, and then allowed to stand at room temperature for 12 h; (4) Add 500 g / L sodium hydroxide solution to the mixture obtained in step (3) to adjust the pH value to 4, then add 200 mL of 8 g / L hexadecyltrimethylammonium bromide solution, stir for 10 min and continue to stand for 6 h, then filter the resulting mixture, and dry the filtered solid at 105° C. for 12 h to obtain urea-formaldehyde resin / SiO2 composite microspheres; calcine the urea-formaldehyde resin / SiO2 composite microspheres in a muffle furnace at 600° C. for 1 h to completely remove the urea-formaldehyde resin, and the obtained silica microspheres are recorded as S-1.

[0061] Example 2 (1) 50 g of retired fan blades were crushed and placed in a fixed bed reactor, and pyrolyzed in a nitrogen atmosphere at 650° C. for 20 min to completely decompose the organic resin component to obtain glass fibers containing residual carbon; then the glass fibers containing residual carbon were oxidized in an air atmosphere at 650° C. for 20 min to completely remove the residual carbon to obtain glass fibers; (2) Grinding the glass fiber obtained in step (1) into a 100-mesh glass fiber powder, mixing 20 g of the glass fiber powder with 30 g of sodium hydroxide, and then calcining at 700° C. for 1 h; grinding the calcined product and mixing it with 200 mL of deionized water, and then magnetically stirring it for 14 h to obtain a suspension; filtering the obtained suspension, and dripping glacial acetic acid into the liquid obtained by filtration until gelation occurs, thereby obtaining a silica sol; (3) 100 mL of the silica sol obtained in step (2) was mixed with 120 mL of urea solution (concentration of 90 g / L) and stirred evenly, and the pH value was adjusted to 3 with glacial acetic acid, and then 70 mL of formaldehyde solution (concentration of 25 wt%) was quickly added to the pH-adjusted mixture, stirred at a rate of 1000 rpm for 1 min, and then allowed to stand at room temperature for 20 h; (4) Add 500 g / L sodium hydroxide solution to the mixture obtained in step (3) to adjust the pH value to 4, then add 180 mL of 9 g / L hexadecyltrimethylammonium bromide solution, stir for 15 min and let stand for 9 h, then filter the mixture, dry the filtered solid at 95 °C for 18 h to obtain urea-formaldehyde resin / SiO2 composite microspheres; calcine the urea-formaldehyde resin / SiO2 composite microspheres in a muffle furnace at 700 °C for 0.5 h to completely remove the urea-formaldehyde resin, and the obtained silica microspheres are recorded as S-2.

[0062] Example 3 (1) 50 g of retired fan blades were crushed and placed in a fixed bed reactor, and pyrolyzed in an argon atmosphere at 450° C. for 50 min to completely decompose the organic resin component to obtain glass fibers containing residual carbon; then the glass fibers containing residual carbon were oxidized in an air atmosphere at 450° C. for 50 min to completely remove the residual carbon to obtain glass fibers; (2) Grinding the glass fiber obtained in step (1) into a 300-mesh glass fiber powder, mixing 25 g of the glass fiber powder with 20 g of sodium hydroxide, and then calcining at 450° C. for 3 h; grinding the calcined product and mixing it with 230 mL of deionized water, and then magnetically stirring it for 10 h to obtain a suspension; filtering the obtained suspension, and dripping glacial acetic acid into the liquid obtained by filtration until gelation occurs, thereby obtaining a silica sol; (3) 100 mL of the silica sol obtained in step (2) was mixed with 175 mL of urea solution (concentration of 70 g / L) and stirred evenly, and the pH value was adjusted to 2 with glacial acetic acid, and then 40 mL of formaldehyde solution (concentration of 40 wt%) was quickly added to the pH-adjusted mixture, stirred at a rate of 650 rpm for 5 min, and then allowed to stand at room temperature for 10 h; (4) Add 450 g / L sodium hydroxide solution to the mixture obtained in step (3) to adjust the pH value to 4, then add 150 mL of 10 g / L hexadecyltrimethylammonium bromide solution, stir for 20 min and let stand for 4 h, then filter the mixture, dry the filtered solid at 120 °C for 9 h to obtain urea-formaldehyde resin / SiO2 composite microspheres; calcine the urea-formaldehyde resin / SiO2 composite microspheres in a muffle furnace at 500 °C for 3 h to completely remove the urea-formaldehyde resin, and the obtained silica microspheres are recorded as S-3.

[0063] Example 4 The method used is substantially the same as that of Example 1, except that, in step (4), 500 g / L of sodium hydroxide solution is added to the mixture obtained in step (3) to adjust the pH value to 2. The obtained silica microspheres are designated as S-4.

[0064] Example 5 The method used is substantially the same as that of Example 1, except that, in step (4), 500 g / L of sodium hydroxide solution is added to the mixture obtained in step (3) to adjust the pH value to 6. The obtained silica microspheres are designated as S-5.

[0065] Example 6 The method used is substantially the same as that of Example 1, except that, in step (4), 500 g / L of sodium hydroxide solution is added to the mixture obtained in step (3) to adjust the pH value to 10. The obtained silica microspheres are designated as S-6.

[0066] Comparative Example 1 The method used is basically the same as that of Example 1, except that the silica sol prepared by using ethyl orthosilicate as the silicon source replaces the silica sol recovered from retired wind turbine blades. The obtained silica microspheres are denoted as D1.

[0067] Application Examples Take 20 g of each of the silica microspheres S-1 to S-6 and D1 prepared in Examples 1-6 and Comparative Example 1, slowly add 12 mL of 500 g / L copper nitrate solution, and then dry the resulting suspension at 105°C. The dried solid is calcined at 500°C for 4 h, and then the calcined solid is further calcined at 400°C in a hydrogen atmosphere for 4 h. The obtained Cu / SiO2 catalysts are recorded as C-1 to C-6 and CD1, respectively.

[0068] Test Example 1 The specific surface areas of the silica microspheres S-1 to S-6 and D1 prepared in Examples 1 to 6 and Comparative Example 1 were tested by the BET method; The average pore diameters of the silica microspheres S-1 to S-6 and D1 prepared in Examples 1 to 6 and Comparative Example 1 were tested by the BJH method; The results are shown in Table 1: Table 1 sample Average pore size (nm) <![CDATA[Specific surface area (m 2 g)]]> S-1 15.6 658 S-2 16.4 646 S-3 16.2 651 S-4 24.5 394 S-5 28.9 285 S-6 38.2 253 D1 19.4 385 As shown in Table 1, the method of the present invention can obtain silica microspheres with large specific surface area and rich pore structure, and the specific surface area can reach up to 658m 2 / g, compared with the silica microspheres prepared with tetraethyl orthosilicate as the silicon source, it has a higher specific surface area, and is conducive to loading and exposing sufficient active sites when used as a catalyst carrier, thereby improving the contact efficiency with the substrate and improving the catalytic performance; by using a base in step (4) to adjust the pH value of the mixture obtained in step (3), the pore structure and specific surface area of ​​the final product can be conveniently adjusted, which is conducive to adjusting the microstructure of the microspheres according to needs and is convenient for practical use.

[0069] Test Example 2 Energy dispersive X-ray fluorescence spectroscopy (EDX) was used to test the main element types and contents in the silica microspheres S-1 to S-6 and D1 prepared in Examples 1-6 and Comparative Example 1, as well as C-1 and CD1 obtained in Preparation Example. The results are shown in Table 2: Table 2 sample <![CDATA[SiO2(%)]]> Cu element (%) Al element (%) Mg element (%) S-1 83.8 12.8 1.4 0.9 S-2 83.1 12.2 1.3 0.7 S-3 83.3 12.5 1.3 0.8 S-4 82.1 11.2 1.1 0.6 S-5 80.4 9.2 1.0 0.6 S-6 74.7 7.3 0.7 0.4 D1 98.3 \ \ \ C-1 74.3 23.7 0.8 0.3 CD1 88.9 11.4 \ \ As can be seen from Table 2, the method of the present invention uses waste fiberglass in waste fan blades as raw materials, and recovers the glass fiber therein as a silicon source to prepare silica microspheres. Even without being loaded, the silica microspheres contain metal elements such as Cu, Mg, and Al. Compared with silica microspheres prepared using tetraethyl orthosilicate as a pure silicon source, the catalyst obtained by loading Cu as a catalyst carrier has a higher Cu content, which is beneficial to further improve the performance of catalyzing furfural hydrogenation to prepare furfuryl alcohol.

[0070] Test Example 3 5 g of each of the Cu / SiO2 catalysts C-1 to C-6 and CD1 obtained in the application examples, as well as the silica microspheres S-1 and D1 prepared in Example 1 and Comparative Example 1, were taken for performance testing of catalytic furfural hydrogenation to prepare furfuryl alcohol. First, the above catalyst or silica microspheres were calcined at 250°C for 2 hours in a mixed gas atmosphere composed of H2 and N2 (H2:N2 volume ratio is 1:5) to activate the catalytic active sites, and then the calcined catalyst or silica microspheres were placed in a reactor, and the furfural hydrogenation reduction reaction was carried out at a reaction temperature of 120°C for 3 hours, and the molar ratio of hydrogen and furfural was added was 10:1; after the reaction was completed, the solid-liquid mixture in the reactor was filtered, and the liquid component was determined by gas chromatograph. The results are shown in Table 3, where the calculation method of the furfural conversion rate is the ratio of the difference in furfural concentration before and after the reaction to the initial concentration of furfural, and the calculation method of furfuryl alcohol selectivity is the ratio of furfuryl alcohol component to all product components.

[0071] Table 3 Element Type Furfural conversion rate Furfuryl alcohol selectivity C-1 94.7% 96.9% C-2 94.6% 95.2% C-3 93.9% 95.0% C-4 90.3% 89.7% C-5 86.2% 86.9% C-6 81.1% 83.3% CD1 76.9% 81.3% S-1 65.2% 78.3% D1 1.9% 16.3% As can be seen from Table 3, the silica microspheres prepared by the method of the present invention are used as carriers to load Cu for catalyzing the hydrogenation of furfural to prepare furfuryl alcohol, and show high catalytic activity. The furfural conversion rate can reach 94.7%, and the furfuryl alcohol selectivity can reach 96.9%. The large specific surface area, rich pore structure and high Cu content of the silica microspheres are important reasons for the high activity of the catalyst. Even without the loading of Cu element, the silica microspheres of the present invention have certain catalytic activity, while the silica microspheres with tetraethyl orthosilicate as the silicon source do not have catalytic activity. This is because the silica microspheres prepared from retired fan blades of the present invention themselves contain metal elements such as Cu, Mg, and Al, and can further improve the catalytic activity of the catalyst when used as Cu-containing catalyst carriers.

[0072] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing silica microspheres using waste glass fiber reinforced plastics, characterized in that: The method comprises the following steps: (1) crushing the waste FRP, performing pyrolysis and oxidation treatments, and recovering the glass fibers; (2) grinding the glass fiber into a glass fiber powder of 100-300 mesh, mixing it with a first alkali, performing a first calcination treatment, mixing the calcined product with water, performing solid-liquid separation, and then mixing the liquid obtained by the solid-liquid separation with a first acid to obtain a silica sol; (3) mixing the silica sol with a urea solution, adjusting the pH to ≤ 4 with a second acid, and then mixing with a formaldehyde solution and reacting; (4) A second base is added to the mixture obtained in the reaction of step (3) to adjust the pH value to 2-10, and then the mixture is mixed with a hexadecyltrimethylammonium bromide solution and allowed to stand, and the mixture obtained after standing is subjected to solid-liquid separation, and then the obtained solid is dried and subjected to a second calcination treatment.

2. The method according to claim 1, characterized in that The waste fiberglass comes from retired wind turbine blades.

3. The method according to claim 1 or 2, characterized in that: In step (1), the pyrolysis treatment is carried out in an inert atmosphere, and the conditions of the pyrolysis treatment include: a temperature of 400-700° C. and a time of 10-60 min; Preferably, the inert atmosphere is a nitrogen atmosphere and / or an argon atmosphere.

4. The method according to any one of claims 1 to 3, characterized in that: In step (1), the oxidation treatment is carried out in an oxygen-containing atmosphere, and the conditions of the oxidation treatment include: a temperature of 400-700° C. and a time of 10-60 min; Preferably, the oxygen-containing atmosphere is an air atmosphere and / or an oxygen atmosphere.

5. The method according to claim 1, characterized in that In step (2), the mass ratio of the glass fiber powder to the first alkali is 1:0.5-2.

6. The method according to claim 1 or 5, characterized in that: In step (2), the first calcination treatment is carried out in an inert atmosphere, and the conditions of the first calcination treatment include: a temperature of 450-750° C. and a time of 1-6 hours; Preferably, the inert atmosphere is a nitrogen atmosphere and / or an argon atmosphere.

7. The method according to claim 1, characterized in that In step (3), the volume ratio of the silica sol to the urea solution is 1:1-3; Preferably, the concentration of the urea solution is 60-100 g / L.

8. The method according to claim 1 or 7, characterized in that: In step (3), the volume ratio of the silica sol to the formaldehyde solution is 1.5-3:1; Preferably, the concentration of the formaldehyde solution is 25-45wt%.

9. The method according to any one of claims 1 or 7-8, characterized in that: In step (3), the reaction conditions include: stirring at 600-1000 rpm for 1-5 min, and then standing for 8-24 h.

10. The method according to claim 1, characterized in that In step (4), the conditions of the second calcination treatment include: temperature of 500-700° C. and time of 0.5-3 h.

11. The method according to claim 1 or 10, characterized in that: In step (4), the volume ratio of the silica sol to the hexadecyltrimethylammonium bromide solution is 1:1.5-3.5; Preferably, the concentration of the hexadecyltrimethylammonium bromide solution is 6-10 g / L.

12. The method according to any one of claims 1 to 11, characterized in that: The first base and the second base are the same or different, and each is at least one of sodium hydroxide, potassium hydroxide and sodium carbonate.

13. The method according to any one of claims 1 to 12, characterized in that: The first acid and the second acid are the same or different, and each is at least one of dilute sulfuric acid, dilute hydrochloric acid and glacial acetic acid.

14. Silica microspheres prepared by the method according to any one of claims 1 to 13.

15. Use of the silica microspheres as claimed in claim 14 as catalyst carriers.

Citation Information

Patent Citations

  • Method for preparing white carbon black by using waste wind turbine blade

    CN115465867A

  • Method for recycling glass fibers through pyrolysis of retired fan blades and regenerated glass fibers obtained through method

    CN115739929A

  • Preparation method of silicon dioxide microspheres with wide distribution pore structure

    CN116282051A