Preparation method and application of eutectic growth FER-MFI molecular sieve

The preparation of FER-MFI molecular sieve by eutectic growth method solves the problems of low catalytic activity and conversion of FER molecular sieve, and achieves high efficiency of diene selectivity and conversion of dienes, which is suitable for catalytic cracking of light hydrocarbons.

CN118929686APending Publication Date: 2024-11-12SHANDONG CHAMBROAD PETROCHEMICALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410982441.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

FER molecular sieve has low catalytic activity and low conversion rate in light hydrocarbon cracking, making it difficult to effectively inhibit the formation of aromatic hydrocarbons, limiting its application depth and breadth.

Method used

FER-MFI molecular sieve was prepared by eutectic growth method, and the MFI seeds were treated with amines through long-chain diamine to form a composite structure of FER and MFI, and the ratio of FER phase and MFI phase was regulated to improve catalytic activity and selectivity.

Benefits of technology

It achieves good performance of improving the selectivity of dienes without reducing the reaction conversion rate, and is suitable for large-scale industrial production and catalyst applications for light hydrocarbon catalytic cracking to produce ethylene and propylene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004956481830000161
    Figure BDA0004956481830000161
  • Figure BDA0004956481830000171
    Figure BDA0004956481830000171
  • Figure BDA0004956481830000172
    Figure BDA0004956481830000172
Patent Text Reader

Abstract

The method is mainly applied to the field of high yield of diene through light hydrocarbon cracking. The invention discloses a preparation method and application of an FER-MFI molecular sieve for eutectic growth. According to the molecular sieve, the ratio of two molecular sieves in eutectic growth is regulated by using alkali amount. The preparation method comprises the following steps: performing amine treatment on seed crystals; mixing and reacting an aluminum source, a silicon source, the ammonium-treated seed crystal and an alkaline substance in water to obtain gel; crystallizing at high temperature, washing, drying and calcining to obtain a molecular sieve solid; and carrying out ion exchange on the molecular sieve solid by using ammonium salt, and calcining to obtain the eutectic growth FER-MFI molecular sieve. The prepared FER-MFI molecular sieve has a special pore structure, and shows excellent diene selectivity by taking the molecular sieve as an active component in a light hydrocarbon cracking catalyst. The light hydrocarbon catalytic cracking catalyst prepared by the invention can improve the diene selectivity without sacrificing the conversion rate, and is especially suitable for the field of refinery light hydrocarbon cracking to produce more dienes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts for cracking light hydrocarbons, and relates to a preparation method and application of a FER-MFI molecular sieve, and in particular to a preparation method and application of a eutectic-grown FER-MFI molecular sieve. Background Art

[0002] Molecular sieves have adjustable pore structures and acidity and are used as catalysts for the catalytic cracking of light hydrocarbons. Researchers have found that molecular sieves with 10-membered ring pore structures, such as FER, ZSM-22, and ZSM-23, show higher ethylene and propylene yields in the cracking of light hydrocarbons. The pore sizes used are (10-MR) and (8-MR) FER molecular sieves, the specific pore sizes are (10-MR) The (10-MR) ZSM-5 zeolite has a stronger pore confinement effect, which may be a way to increase the yield of light olefins while suppressing aromatics. Compared with other zeolites such as ZSM-5, FER has a stronger selectivity for the formation of olefins, but FER generally exhibits lower catalytic activity. This means that FER zeolites have low conversion and high diene selectivity.

[0003] Therefore, how to find a more appropriate way to solve the above-mentioned problems of FER molecular sieves and further broaden the depth and breadth of their applications has become one of the focuses of widespread attention of many front-line researchers in the industry. Summary of the invention

[0004] In view of this, the technical problem to be solved by the present invention is to provide a preparation method and application of FER-MFI molecular sieve, in particular, a preparation method of eutectic-grown FER-MFI molecular sieve. The present invention prepares and synthesizes eutectic-grown FER-MFI molecular sieve, which is particularly applicable to catalysts for catalytic cracking of light hydrocarbons to produce ethylene and propylene, achieving good performance of not reducing reaction conversion rate and improving diene selectivity. Moreover, the preparation method has mild conditions, simple process, good controllability, and is more suitable for promotion and application of large-scale industrial production.

[0005] The present invention provides a method for preparing a FER-MFI molecular sieve, comprising the following steps:

[0006] 1) mixing an aluminum source, a silicon source, a diamine-modified seed crystal, an alkaline substance and water to obtain a gel;

[0007] 2) crystallizing the gel obtained in the above step and then calcining it to obtain a molecular sieve solid;

[0008] 3) The molecular sieve solid obtained in the above step is subjected to ion exchange with ammonium salt and then calcined again to obtain the FER-MFI molecular sieve.

[0009] Preferably, the diamine includes a C6-C10 long-chain diamine;

[0010] The C6-C10 long-chain diamine includes one or more of hexamethylenediamine, heptamethylenediamine, octanediamine and nonamethylenediamine;

[0011] The preparation steps of the diamine-modified seed crystals include: mixing the seed crystals with diamine and then performing amine treatment to obtain the diamine-modified seed crystals;

[0012] The temperature of the amine treatment is 80 to 120°C;

[0013] The amine treatment time is 8 to 12 hours;

[0014] The molar ratio of the seed crystal to the diamine is (1-2): (5-10);

[0015] The seed crystals are MFI phase seed crystals.

[0016] Preferably, the aluminum source is one or more of aluminum hydroxide, sodium aluminate and pseudo-boehmite;

[0017] The silicon source is one or more of silica gel, sodium silicate and silica sol;

[0018] The silicon source and aluminum source are SiO 2 and Al 2 O 3 The molar ratio of silicon source to aluminum source is (2-3): (0.1-0.2);

[0019] The alkaline substance is one or more of an organic base and an inorganic base;

[0020] The organic base includes one or more of tetrapropylammonium hydroxide, tetraethylammonium hydroxide, triethylamine and n-butylamine;

[0021] The inorganic base includes one or more of potassium hydroxide, sodium hydroxide, sodium carbonate and sodium bicarbonate.

[0022] Preferably, the aluminum source and the alkaline substance have a molar ratio of (1-2): (0.1-1.5) based on Al and OH radicals;

[0023] The aluminum source is calculated as Al, and the molar ratio of the aluminum source to water is (1-2): (100-200);

[0024] The diamine modified seed crystal and the silicon source and the aluminum source are SiO 2 and Al 2 O3 The seed crystal and SiO 2 +Al 2 O 3 The mass ratio of the total mass is (0.05-5):100;

[0025] The step 1) specifically comprises the following steps:

[0026] 11) mixing an aluminum source, an alkaline substance and water to obtain a solution;

[0027] 12) continuing to mix the solution obtained in the above step with a silicon source to obtain a first gel;

[0028] 13) The first gel obtained in the above step and the diamine-modified seed crystals are mixed again to obtain a gel.

[0029] Preferably, the seed crystals are ZSM-5 molecular sieve seed crystals and / or S-1 molecular sieve seed crystals;

[0030] The crystallization further includes a washing and / or drying step;

[0031] The crystallization temperature is 160-180°C;

[0032] The crystallization time is 24 to 72 hours;

[0033] The calcination temperature is 500-700°C;

[0034] The calcination time is 3 to 5 hours.

[0035] Preferably, the ammonium salt is one or more of ammonium chloride, ammonium nitrate and ammonium acetate;

[0036] The mass ratio of the ammonium salt to the molecular sieve solid is 1:(4-10);

[0037] The re-calcination temperature is 500-700°C;

[0038] The re-calcination time is 3 to 5 hours.

[0039] Preferably, the FER-MFI molecular sieve is a eutectic-grown FER-MFI molecular sieve;

[0040] The FER-MFI molecular sieve has a composite crystal structure of FER and MFI;

[0041] The FER-MFI molecular sieve has a composite structure of FER micro-nano sheets and MFI nano-blocks;

[0042] The FER micro-nanosheet has a radial dimension of 0.5 to 2 μm and a thickness of 20 to 60 nm;

[0043] The particle size of the MFI nanoblock is 50-100nm*60-200nm;

[0044] In the FER-MFI molecular sieve, the mass content of the MFI phase is 80% to 98%.

[0045] The present invention also provides the use of the FER-MFI molecular sieve prepared by the preparation method described in any one of the above technical solutions in the field of light hydrocarbon cracking.

[0046] Preferably, the application includes the use of FER-MFI molecular sieve as a catalyst in the cracking process of light hydrocarbons;

[0047] The application is specifically the application of the FER-MFI molecular sieve active component, kaolin and a binder combined as a composite catalyst;

[0048] In the composite catalyst, the mass content of the FER-MFI molecular sieve active component is 30% to 50%;

[0049] In the composite catalyst, the mass content of kaolin is 20% to 40%.

[0050] Preferably, the composite catalyst is obtained by mixing, ball milling and molding FER-MFI molecular sieve active components, kaolin and a binder;

[0051] The binder includes one or more of alumina sol, silica sol, acidified pseudo-boehmite, water glass and aluminum phosphate;

[0052] The light hydrocarbon raw material for cracking light hydrocarbons includes one or more of C5-C8 alkanes, olefins and aromatics;

[0053] The reaction device of the light hydrocarbon cracking process includes a fixed fluidized bed reactor.

[0054] The present invention provides a method for preparing a FER-MFI molecular sieve, comprising the following steps: firstly, an aluminum source, a silicon source, a diamine modified seed crystal, an alkaline substance and water are mixed and reacted to obtain a gel; then, the gel obtained in the above steps is crystallized and then calcined to obtain a molecular sieve solid; finally, an ammonium salt is used to perform ion exchange on the molecular sieve solid obtained in the above steps, and then calcined again to obtain a FER-MFI molecular sieve. Compared with the prior art, the present invention designs a method for preparing a FER-MFI molecular sieve with specific processing steps and parameter control, by using a long-chain diamine to perform amine treatment on the MFI seed crystal, and using the weak alkalinity of the long-chain diamine to etch the MFI seed crystal. The amine head of the long-chain diamine is embedded in the etched seed crystal and connected to the seed crystal. Since a seed crystal is connected to each end of the long-chain diamine, the molecular sieve forms a layered structure during the crystallization process, which is conducive to the formation of a guided FER phase; while the seed crystal not connected to the long-chain diamine is conducive to the formation of a guided MFI phase. Therefore, the FER-MFI eutectic molecular sieve is synthesized by using only MFI seeds treated with amines, and the present invention also finds that the ratio of the FER phase and the MFI phase in the FER-MFI eutectic molecular sieve can be regulated by varying the amount of alkali in the synthetic gel.

[0055] The present invention synthesizes a eutectic FER-MFI molecular sieve, further explores the optimal ratio of the two, and synthesizes a series of molecular sieves, achieving good performance of improving diene selectivity without reducing the reaction conversion rate. The present invention uses a FER-MFI molecular sieve prepared by eutectic growth, and a molecular sieve having both a FER structure and an MFI structure as an active component of a light hydrocarbon cracking reaction catalyst, and uses it as a catalyst for catalytic cracking of light hydrocarbons to produce ethylene and propylene, which is beneficial to improving the conversion rate and diene selectivity.

[0056] The present invention overcomes the limitations of a single molecular sieve, and after combining two molecular sieves of different structures, it plays a dual role, thereby improving the activity and diene selectivity of the reaction of catalytic cracking of light hydrocarbons to produce ethylene and propylene, which is of great significance. In addition, the preparation method has mild conditions, simple process, good controllability, strong stability, and is more suitable for promotion and application of large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 X-ray diffraction spectra of molecular sieve powders prepared in the examples and comparative examples of the present invention;

[0058] Figure 2 This is a scanning electron microscope photo of the molecular sieve prepared in the embodiment of the present invention;

[0059] Figure 3 This is a scanning electron microscope photograph of the molecular sieve prepared in the comparative example of the present invention. DETAILED DESCRIPTION

[0060] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention.

[0061] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0062] There is no particular limitation on the purity of all raw materials in the present invention. The present invention preferably uses analytically pure raw materials or raw materials of conventional purity used in the field of light hydrocarbon cracking catalyst preparation.

[0063] The present invention provides a method for preparing a FER-MFI molecular sieve, comprising the following steps:

[0064] 1) mixing an aluminum source, a silicon source, a diamine-modified seed crystal, an alkaline substance and water to obtain a gel;

[0065] 2) crystallizing the gel obtained in the above step and then calcining it to obtain a molecular sieve solid;

[0066] 3) The molecular sieve solid obtained in the above step is subjected to ion exchange with ammonium salt and then calcined again to obtain the FER-MFI molecular sieve.

[0067] The invention firstly mixes aluminum source, silicon source, diamine modified seed crystal, alkaline substance and water to obtain gel.

[0068] In the present invention, the diamine preferably includes a C6-C10 long-chain diamine, and more preferably a C7-C8 long-chain diamine.

[0069] In the present invention, the C6-C10 long-chain diamine preferably includes one or more of hexamethylenediamine, heptamethylenediamine, octanediamine and nonamethylenediamine, and more preferably hexamethylenediamine, heptamethylenediamine, octanediamine or nonamethylenediamine.

[0070] In the present invention, the preparation step of the diamine-modified seed crystals includes: mixing the seed crystals with diamine and then subjecting the mixture to amine treatment to obtain the diamine-modified seed crystals.

[0071] In the present invention, the temperature of the amine treatment is preferably 80 to 120°C, more preferably 90 to 110°C.

[0072] In the present invention, the time of the amine treatment is preferably 8 to 12 hours, more preferably 9 to 11 hours.

[0073] In the present invention, the molar ratio of the seed crystal to the diamine is preferably (1-2):(5-10), or (1.2-1.8):(5-10), or (1.4-1.6):(5-10), or (1-2):(6-9), or (1-2):(7-8).

[0074] In the present invention, the seed crystals are preferably MFI phase seed crystals.

[0075] In the present invention, the aluminum source is preferably one or more of aluminum hydroxide, sodium aluminate and pseudo-boehmite, more preferably aluminum hydroxide, sodium aluminate or pseudo-boehmite.

[0076] In the present invention, the silicon source is preferably one or more of silica gel, sodium silicate and silica sol, more preferably silica gel, sodium silicate or silica sol.

[0077] In the present invention, the silicon source and the aluminum source are SiO 2 and Al 2 O 3 The molar ratio of the silicon source to the aluminum source is preferably (2-3):(0.1-0.2), more preferably (2.2-2.8):(0.12-0.18), and more preferably (2.4-2.6):(0.14-0.16).

[0078] In the present invention, the alkaline substance is preferably one or more of an organic base and an inorganic base, and more preferably one of an organic base or an inorganic base.

[0079] In the present invention, the organic base preferably includes one or more of tetrapropylammonium hydroxide, tetraethylammonium hydroxide, triethylamine and n-butylamine, and more preferably tetrapropylammonium hydroxide, tetraethylammonium hydroxide, triethylamine or n-butylamine.

[0080] In the present invention, the inorganic base preferably includes one or more of potassium hydroxide, sodium hydroxide, sodium carbonate and sodium bicarbonate, and more preferably potassium hydroxide, sodium hydroxide, sodium carbonate or sodium bicarbonate.

[0081] In the present invention, the molar ratio of the aluminum source and the alkaline substance, calculated as Al and OH radical, is preferably (1-2):(0.1-1.5), more preferably (1.2-1.8):(0.4-1.1), and more preferably (1.4-1.6):(0.7-0.8).

[0082] In the present invention, the aluminum source is calculated as Al, and the molar ratio of the aluminum source to water is preferably (1-2): (100-200), more preferably (1.2-1.8): (120-180), and more preferably (1.4-1.6): (140-160).

[0083] In the present invention, the crystalline diamine modified seed crystal and the silicon source and the aluminum source are SiO 2 and Al 2 O 3 The seed crystal and SiO 2 +Al 2 O 3 The mass ratio of the total mass is preferably (0.05 to 5):100, more preferably (0.5 to 4):100, and even more preferably (1.5 to 3):100.

[0084] In the present invention, the seed crystals are preferably ZSM-5 molecular sieve seed crystals and / or S-1 molecular sieve seed crystals, and more preferably ZSM-5 molecular sieve seed crystals or S-1 molecular sieve seed crystals.

[0085] In the present invention, the step 1) preferably comprises the following steps:

[0086] 11) mixing an aluminum source, an alkaline substance and water to obtain a solution;

[0087] 12) continuing to mix the solution obtained in the above step with a silicon source to obtain a first gel;

[0088] 13) The first gel obtained in the above step and the diamine-modified seed crystals are mixed again to obtain a gel.

[0089] In the present invention, the gel obtained in the above steps is crystallized and then calcined to obtain a molecular sieve solid.

[0090] In the present invention, the crystallization preferably further comprises a washing and / or drying step, more preferably a washing and drying step.

[0091] In the present invention, the crystallization temperature is preferably 160-180°C, more preferably 164-176°C, and more preferably 168-172°C.

[0092] In the present invention, the crystallization time is preferably 24 to 72 hours, more preferably 34 to 62 hours, and more preferably 44 to 52 hours.

[0093] In the present invention, the calcination temperature is preferably 500-700°C, more preferably 540-660°C, and more preferably 580-620°C.

[0094] In the present invention, the calcination time is preferably 3 to 5 hours, more preferably 3.4 to 4.6 hours, and more preferably 3.8 to 4.2 hours.

[0095] In the present invention, the molecular sieve solid obtained in the above steps is ion exchanged with ammonium salt and then calcined again to obtain the FER-MFI molecular sieve.

[0096] In the present invention, the ammonium salt is preferably one or more of ammonium chloride, ammonium nitrate and ammonium acetate, more preferably ammonium chloride, ammonium nitrate or ammonium acetate.

[0097] In the present invention, the mass ratio of the ammonium salt to the molecular sieve solid is preferably 1:(4-10), more preferably 1:(5-9), and more preferably 1:(6-8).

[0098] In the present invention, the temperature of the re-calcination is preferably 500-700°C, more preferably 540-660°C, and more preferably 580-620°C.

[0099] In the present invention, the re-calcination time is preferably 3 to 5 hours, more preferably 3.4 to 4.6 hours, and more preferably 3.8 to 4.2 hours.

[0100] In the present invention, the FER-MFI molecular sieve is preferably a eutectic-grown FER-MFI molecular sieve.

[0101] In the present invention, the FER-MFI molecular sieve preferably has a composite crystal phase structure of FER and MFI.

[0102] In the present invention, the FER-MFI molecular sieve preferably has a structure of FER micro-nano sheets and MFI nano-blocks doped and composited.

[0103] In the present invention, the radial dimension of the FER micro-nanosheet is preferably 0.5-2 μm, the thickness is preferably 20-60 nm, the radial dimension is more preferably 0.8-1.7 μm, the thickness is preferably 25-55 nm, the radial dimension is more preferably 1.1-1.4 μm, the thickness is preferably 30-50 nm.

[0104] In the present invention, the particle size of the MFI nanoblock is preferably 50-100 nm*60-200 nm, more preferably 60-90 nm*90-170 nm, and more preferably 70-80 nm*120-140 nm.

[0105] In the present invention, in the FER-MFI molecular sieve, the mass content of the MFI phase is preferably 80% to 98%, more preferably 84% to 94%, and more preferably 88% to 90%.

[0106] The present invention provides the application of the FER-MFI molecular sieve prepared by the preparation method described in any one of the above technical solutions in the field of light hydrocarbon cracking.

[0107] In the present invention, the application preferably includes the application of FER-MFI molecular sieve as a catalyst in the light hydrocarbon cracking process.

[0108] In the present invention, the application is preferably the application of the FER-MFI molecular sieve active component, kaolin and a binder combined as a composite catalyst.

[0109] In the present invention, in the composite catalyst, the mass content of the FER-MFI molecular sieve active component is preferably 30% to 50%, more preferably 34% to 46%, and more preferably 38% to 42%.

[0110] In the present invention, the mass content of kaolin in the composite catalyst is preferably 20% to 40%, more preferably 24% to 36%, and more preferably 28% to 32%.

[0111] In the present invention, the composite catalyst is preferably obtained by mixing, ball milling and molding the FER-MFI molecular sieve active component, kaolin and a binder.

[0112] In the present invention, the binder preferably includes one or more of alumina sol, silica sol, acidified pseudo-boehmite, water glass and aluminum phosphate, and more preferably includes alumina sol, silica sol, acidified pseudo-boehmite, water glass or aluminum phosphate.

[0113] In the present invention, the light hydrocarbon raw material for light hydrocarbon cracking preferably includes one or more of C5-C8 alkanes, olefins and aromatics, more preferably C6-C7 alkanes, olefins or aromatics.

[0114] In the present invention, the reaction device of the light hydrocarbon cracking process preferably includes a fixed fluidized bed reactor.

[0115] The present invention is to complete and refine the overall technical solution, better ensure the structure and composition of the FER-MFI eutectic molecular sieve, and further improve the catalytic activity of the FER-MFI molecular sieve in catalyzing the cracking of light hydrocarbons to produce ethylene and propylene. The preparation method and application of the above-mentioned FER-MFI molecular sieve may specifically include the following contents:

[0116] A method for preparing a eutectic-grown FER-MFI molecular sieve comprises the following steps:

[0117] mixing the seed crystals and the diamine to perform an amine treatment;

[0118] An aluminum source, a silicon source, amine-treated seed crystals and an alkaline substance are mixed and reacted in water to obtain a gel;

[0119] The gel is crystallized at high temperature, washed, dried and calcined to obtain a molecular sieve solid; an ammonium salt is used to perform ion exchange on the molecular sieve solid, and then calcined to obtain a FER-MFI molecular sieve.

[0120] Specifically, the diamine is one or more of hexamethylenediamine, heptamethylenediamine, octanediamine, and nonanediamine.

[0121] Specifically, the seed crystals are commercially available ZSM-5 molecular sieve and / or S-1 molecular sieve seed crystals.

[0122] Specifically, the aluminum source is one or more of aluminum hydroxide, sodium aluminate and pseudo-boehmite.

[0123] Specifically, the silicon source is one or more of silica gel, sodium silicate, and silica sol.

[0124] Specifically, the alkaline substance includes one or more of an organic base and an inorganic base.

[0125] Specifically, the SiO 2 :Al 2 O 3 The molar ratio is 2-3:0.1-0.2.

[0126] Specifically, the molar ratio of sodium aluminate:OH-:water is 1-2:0.1-1.5:100-200.

[0127] Specifically, seed crystal: (SiO 2 +Al 2 O 3 ) mass ratio 0.05~5wt%.

[0128] Specifically, the amine treatment temperature is 80-120°C.

[0129] Specifically, the amine treatment time is 8-12 hours.

[0130] Specifically, the crystallization temperature is 160-180° C. and the time is 24-72 hours.

[0131] Specifically, the calcination temperature after crystallization is 500-700° C. and the calcination time is 3-5 hours.

[0132] Specifically, the ammonium salt is one or more of ammonium chloride, ammonium nitrate and ammonium acetate; the calcination temperature after the ion exchange is 500-700° C. and the time is 3-5 hours.

[0133] Furthermore, a method for preparing a eutectic-grown FER-MFI molecular sieve of the present invention is as follows:

[0134] (1) The seed crystals and diamine are mixed in a certain ratio and pretreated at a certain temperature to obtain amine-treated seed crystals.

[0135] (2) Sodium aluminate, alkali and water are mixed in a certain proportion and stirred evenly to obtain solution A.

[0136] (3) Add silica gel to solution A to obtain gel B.

[0137] (4) Add a certain amount of amine-treated seed crystals to gel B to obtain gel C.

[0138] (5) Transfer gel C to a reactor and crystallize it at a certain temperature for a certain period of time.

[0139] (6) Washing, drying and calcining the crystallized molecular sieve to obtain solid a.

[0140] (7) Solid a is ion exchanged with an ammonium salt, and then calcined at a certain temperature and time to obtain solid b.

[0141] (8) Solid b is used as the active component of the catalyst, mixed evenly with a certain amount of kaolin and a binder, and then ball-milled and atomized to form the solid.

[0142] (9) The catalyst is calcined and the obtained sample is subjected to light hydrocarbon cracking reaction evaluation in a fixed fluidized bed reactor.

[0143] Specifically, the seed crystal in step (1) is one of ZSM-5 molecular sieve and / or S-1 molecular sieve or a mixture thereof.

[0144] Specifically, the diamine is one or more of hexamethylenediamine, heptamethylenediamine, octanediamine, and nonanediamine.

[0145] Specifically, the molar ratio of seed crystal: diamine = 1-2: 5-10.

[0146] Specifically, the pretreatment temperature is 80-120° C., and the pretreatment time is 8-12 hours.

[0147] Specifically, the molar ratio of sodium aluminate: OH-: water in step (2) is 1-2: 0.1-1.5: 100-200. The base includes one or more of an organic base and an inorganic base.

[0148] Specifically, the Al in step (3) 2 O 3 :SiO 2 The molar ratio is 0.1-0.2:2-3.

[0149] Specifically, the pre-treated seed crystals in step (4) (measured by seed crystal mass): (SiO 2 +Al 2 O 3 ) mass ratio 0.05-5wt%.

[0150] Specifically, the temperature in step (5) is 160-180°C and the time is 24-72h.

[0151] Specifically, the calcination temperature in step (6) is 500-700° C. and the calcination time is 3-5 hours.

[0152] Specifically, the ammonium salt in step (7) is one or more of ammonium chloride, ammonium nitrate, and ammonium acetate, and the calcination temperature is 500-700° C. and the time is 3-5 hours.

[0153] Specifically, the kaolin in step (8) is 20-40%; the molecular sieve is 30-50%; the binder is 10-30%, and the binder includes but is not limited to a mixture of one or more of aluminum sol, silica sol, acidified pseudo-boehmite, water glass, and aluminum phosphate.

[0154] Specifically, the catalytic cracking raw material in step (9) is one of C5-C8 alkanes, olefins, aromatics or a mixture thereof.

[0155] The present invention provides a FER-MFI molecular sieve obtained by the preparation method described in any one of the above technical solutions, and the FER-MFI molecular sieve has a composite crystal phase structure of FER and MFI.

[0156] The present invention provides a light hydrocarbon cracking catalyst, which uses the FER-MFI molecular sieve described in the above technical solution as an active component.

[0157] The present invention provides the use of the light hydrocarbon cracking catalyst as described in the above technical solution in light hydrocarbon cracking.

[0158] The present invention discloses a preparation method and application of a eutectic FER-MFI molecular sieve. The preparation method of the molecular sieve comprises: treating a seed with amine; mixing an aluminum source, a silicon source, an amine-treated seed and an alkaline substance in water to obtain a gel; crystallizing at a high temperature, washing, drying and calcining to obtain a molecular sieve solid; using an ammonium salt to perform ion exchange on the molecular sieve solid, and then calcining to obtain a eutectic FER-MFI molecular sieve. The present invention is mainly used in the field of catalytic cracking and high production of propylene in petrochemical industry. The FER-MFI molecular sieve prepared by the present invention has a special pore structure, and the molecular sieve is used as an active ingredient in a light hydrocarbon cracking catalyst, showing excellent diene selectivity. The light hydrocarbon catalytic cracking catalyst prepared by the present invention can improve diene selectivity without sacrificing conversion rate, and is particularly suitable for the field of high production of dienes in light hydrocarbon cracking in refineries.

[0159] The above content of the present invention provides a preparation method and application of FER-MFI molecular sieve, and particularly relates to a preparation method and application of a eutectic FER-MFI molecular sieve. The preparation method of the FER-MFI molecular sieve designed by the present invention with specific processing steps and parameter control is to treat the MFI seed with amine by using a long-chain diamine, and to etch the MFI seed with weak alkalinity of the long-chain diamine. The amine head of the long-chain diamine is embedded in the etched seed and connected to the seed. Since a seed is connected to each end of the long-chain diamine, the molecular sieve forms a layered structure during the crystallization process, which is conducive to the formation of the FER phase; while the seed without the long-chain diamine is conducive to the formation of the MFI phase. Therefore, the FER-MFI eutectic molecular sieve is synthesized by only using the MFI seed treated with amine, and the present invention also finds that the ratio of the FER phase and the MFI phase in the FER-MFI eutectic molecular sieve can be regulated by the different amounts of alkali in the synthetic gel.

[0160] The present invention synthesizes a eutectic FER-MFI molecular sieve, further explores the optimal ratio of the two, and synthesizes a series of molecular sieves, achieving good performance of improving diene selectivity without reducing the reaction conversion rate. The present invention uses a FER-MFI molecular sieve prepared by eutectic growth, and a molecular sieve having both a FER structure and an MFI structure as an active component of a light hydrocarbon cracking reaction catalyst, and uses it as a catalyst for catalytic cracking of light hydrocarbons to produce ethylene and propylene, which is beneficial to improving the conversion rate and diene selectivity.

[0161] The present invention overcomes the limitations of a single molecular sieve, and after combining two molecular sieves of different structures, it plays a dual role, thereby improving the activity and diene selectivity of the reaction of catalytic cracking of light hydrocarbons to produce ethylene and propylene, which is of great significance. In addition, the preparation method has mild conditions, simple process, good controllability, strong stability, and is more suitable for promotion and application of large-scale industrial production.

[0162] In order to further illustrate the present invention, the preparation method and application of a FER-MFI molecular sieve provided by the present invention are described in detail below in combination with examples. However, it should be understood that these examples are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operating processes are given only to further illustrate the characteristics and advantages of the present invention, rather than to limit the claims of the present invention, and the protection scope of the present invention is not limited to the following examples.

[0163] Example 1

[0164] (1) 1 mol of seed crystals and 5 mol of diamine were mixed and pretreated at 100° C. for 10 h to obtain amine-treated seed crystals.

[0165] (2) Add 1 mol of sodium aluminate and 1.5 mol of sodium hydroxide to 100 mol of water and stir evenly to obtain solution A.

[0166] (3) Add 15 mol of silica gel to solution A to obtain gel B.

[0167] (4) Add 0.05 wt % of amine-treated seed crystals (calculated based on the actual amount of seed crystals) to gel B to obtain gel C.

[0168] (5) Gel C was transferred to a reactor and crystallized at 170 °C for 24 h.

[0169] (6) The crystallized molecular sieve was washed with deionized water until neutral, dried at 60° C. for 8 h, and calcined at 500° C. for 4 h to obtain solid a.

[0170] (7) Using an ammonium chloride solution with a concentration of 0.1 mol / L, solid a was ion exchanged at a solid-liquid ratio of 1:10, and then calcined at 500° C. for 4 h to obtain solid b.

[0171] (8) With solid b as the active component of the catalyst, 600 g of kaolin, 130 g of aluminum sol, 70 g of phosphoric acid, 400 g of molecular sieve, and 130 g of silica sol are added in the order of mixing and stirring to form a slurry. After ball milling, the slurry is spray-formed in a spray dryer.

[0172] (9) The prepared microsphere particles were calcined at 500 °C for 2 h, and the obtained samples were evaluated using a fixed fluidized bed reactor.

[0173] See Table 1, which shows the molecular sieve prepared in Example 1 of the present invention.

[0174] Example 2

[0175] (1) 1 mol of seed crystals and 5 mol of diamine were mixed and pretreated at 100° C. for 10 h to obtain amine-treated seed crystals.

[0176] (2) Add 1 mol of sodium aluminate and 1 mol of sodium hydroxide to 100 mol of water and stir evenly to obtain solution A.

[0177] (3) Add 15 mol of silica gel to solution A to obtain gel B.

[0178] (4) Add 0.05 wt % of amine-treated seed crystals (calculated based on the actual amount of seed crystals) to gel B to obtain gel C.

[0179] (5) Gel C was transferred to a reactor and crystallized at 170 °C for 24 h.

[0180] (6) The crystallized molecular sieve was washed with deionized water until neutral, dried at 60° C. for 8 h, and calcined at 500° C. for 4 h to obtain solid a.

[0181] (7) Using an ammonium chloride solution with a concentration of 0.1 mol / L, solid a was ion exchanged at a solid-liquid ratio of 1:10, and then calcined at 500° C. for 4 h to obtain solid b.

[0182] (8) With solid b as the active component of the catalyst, 600 g of kaolin, 130 g of aluminum sol, 70 g of phosphoric acid, 400 g of molecular sieve, and 130 g of silica sol are added in the order of mixing and stirring to form a slurry. After ball milling, the slurry is spray-formed in a spray dryer.

[0183] (9) The prepared microsphere particles were calcined at 500 °C for 2 h, and the obtained samples were evaluated using a fixed fluidized bed reactor.

[0184] Example 3

[0185] (1) 1 mol of seed crystals and 5 mol of diamine were mixed and pretreated at 100° C. for 10 h to obtain amine-treated seed crystals.

[0186] (2) Add 1 mol of sodium aluminate and 0.8 mol of sodium hydroxide to 100 mol of water and stir evenly to obtain solution A.

[0187] (3) Add 15 mol of silica gel to solution A to obtain gel B.

[0188] (4) Add 0.05 wt % of amine-treated seed crystals (calculated based on the actual amount of seed crystals) to gel B to obtain gel C.

[0189] (5) Gel C was transferred to a reactor and crystallized at 170 °C for 24 h.

[0190] (6) The crystallized molecular sieve was washed with deionized water until neutral, dried at 60° C. for 8 h, and calcined at 500° C. for 4 h to obtain solid a.

[0191] (7) Using an ammonium chloride solution with a concentration of 0.1 mol / L, solid a was ion exchanged at a solid-liquid ratio of 1:10, and then calcined at 500° C. for 4 h to obtain solid b.

[0192] (8) With solid b as the active component of the catalyst, 600 g of kaolin, 130 g of aluminum sol, 70 g of phosphoric acid, 400 g of molecular sieve, and 130 g of silica sol are added in the order of mixing and stirring to form a slurry. After ball milling, the slurry is spray-formed in a spray dryer.

[0193] (9) The prepared microsphere particles were calcined at 500 °C for 2 h, and the obtained samples were evaluated using a fixed fluidized bed reactor.

[0194] Example 4

[0195] (1) 1 mol of seed crystals and 5 mol of diamine were mixed and pretreated at 100° C. for 10 h to obtain amine-treated seed crystals.

[0196] (2) Add 1 mol of sodium aluminate and 0.5 mol of sodium hydroxide to 100 mol of water and stir evenly to obtain solution A.

[0197] (3) Add 15 mol of silica gel to solution A to obtain gel B.

[0198] (4) Add 0.05 wt % of amine-treated seed crystals (calculated based on the actual amount of seed crystals) to gel B to obtain gel C.

[0199] (5) Gel C was transferred to a reactor and crystallized at 170 °C for 24 h.

[0200] (6) The crystallized molecular sieve was washed with deionized water until neutral, dried at 60° C. for 8 h, and calcined at 500° C. for 4 h to obtain solid a.

[0201] (7) Using an ammonium chloride solution with a concentration of 0.1 mol / L, solid a was ion exchanged at a solid-liquid ratio of 1:10, and then calcined at 500° C. for 4 h to obtain solid b.

[0202] (8) With solid b as the active component of the catalyst, 600 g of kaolin, 130 g of aluminum sol, 70 g of phosphoric acid, 400 g of molecular sieve, and 130 g of silica sol are added in the order of mixing and stirring to form a slurry. After ball milling, the slurry is spray-formed in a spray dryer.

[0203] (9) The prepared microsphere particles were calcined at 500 °C for 2 h, and the obtained samples were evaluated using a fixed fluidized bed reactor.

[0204] Example 5

[0205] (1) 1 mol of seed crystals and 5 mol of diamine were mixed and pretreated at 100° C. for 10 h to obtain amine-treated seed crystals.

[0206] (2) Add 1 mol of sodium aluminate and 0.3 mol of sodium hydroxide to 100 mol of water and stir evenly to obtain solution A.

[0207] (3) Add 15 mol of silica gel to solution A to obtain gel B.

[0208] (4) Add 0.05 wt % of amine-treated seed crystals (calculated based on the actual amount of seed crystals) to gel B to obtain gel C.

[0209] (5) Gel C was transferred to a reactor and crystallized at 170 °C for 24 h.

[0210] (6) The crystallized molecular sieve was washed with deionized water until neutral, dried at 60° C. for 8 h, and calcined at 500° C. for 4 h to obtain solid a.

[0211] (7) Using an ammonium chloride solution with a concentration of 0.1 mol / L, solid a was ion exchanged at a solid-liquid ratio of 1:10, and then calcined at 500° C. for 4 h to obtain solid b.

[0212] (8) With solid b as the active component of the catalyst, 600 g of kaolin, 130 g of aluminum sol, 70 g of phosphoric acid, 400 g of molecular sieve, and 130 g of silica sol are added in the order of mixing and stirring to form a slurry. After ball milling, the slurry is spray-formed in a spray dryer.

[0213] (9) The prepared microsphere particles were calcined at 500 °C for 2 h, and the obtained samples were evaluated using a fixed fluidized bed reactor.

[0214] Example 6

[0215] (1) 1 mol of seed crystals and 5 mol of diamine were mixed and pretreated at 100° C. for 10 h to obtain amine-treated seed crystals.

[0216] (2) Add 1 mol of sodium aluminate and 0.1 mol of sodium hydroxide to 100 mol of water and stir evenly to obtain solution A.

[0217] (3) Add 15 mol of silica gel to solution A to obtain gel B.

[0218] (4) Add 0.05 wt % of amine-treated seed crystals (calculated based on the actual amount of seed crystals) to gel B to obtain gel C.

[0219] (5) Gel C was transferred to a reactor and crystallized at 170 °C for 24 h.

[0220] (6) The crystallized molecular sieve was washed with deionized water until neutral, dried at 60° C. for 8 h, and calcined at 500° C. for 4 h to obtain solid a.

[0221] (7) Using an ammonium chloride solution with a concentration of 0.1 mol / L, solid a was ion exchanged at a solid-liquid ratio of 1:10, and then calcined at 500° C. for 4 h to obtain solid b.

[0222] (8) With solid b as the active component of the catalyst, 600 g of kaolin, 130 g of aluminum sol, 70 g of phosphoric acid, 400 g of molecular sieve, and 130 g of silica sol are added in the order of mixing and stirring to form a slurry. After ball milling, the slurry is spray-formed in a spray dryer.

[0223] (9) The prepared microsphere particles were calcined at 500 °C for 2 h, and the obtained samples were evaluated using a fixed fluidized bed reactor.

[0224] Comparative Example 1

[0225] (1) Add 1 mol of sodium aluminate and 2 mol of sodium hydroxide to 100 mol of water and stir evenly to obtain solution A.

[0226] (2) Add 15 mol of silica gel to solution A to obtain gel B.

[0227] (3) Add 0.05 wt% of untreated S-1 seed crystals to gel B to obtain gel C.

[0228] (4) Gel C was transferred to a reactor and crystallized at 170°C for 24 h.

[0229] (5) The crystallized molecular sieve was washed with deionized water until neutral, dried at 60° C. for 8 h, and calcined at 500° C. for 4 h to obtain solid a.

[0230] (6) Using an ammonium chloride solution with a concentration of 0.1 mol / L, solid a was ion exchanged at a solid-liquid ratio of 1:10, and then calcined at 500° C. for 4 h to obtain solid b.

[0231] (7) With solid b as the active component of the catalyst, 600 g of kaolin, 130 g of aluminum sol, 70 g of phosphoric acid, 400 g of molecular sieve, and 130 g of silica sol are added in the order of mixing and stirring to form a slurry. After ball milling the slurry, it is spray-formed in a spray dryer.

[0232] (8) The prepared microsphere particles were calcined at 500 °C for 2 h, and the obtained samples were evaluated using a fixed fluidized bed reactor.

[0233] Example 7

[0234] See also Figure 1 , Figure 1 The X-ray diffraction spectra of the molecular sieve powders prepared in the examples and comparative examples of the present invention are shown.

[0235] See also Figure 2 , Figure 2 This is a scanning electron microscope photograph of the molecular sieve prepared in the embodiment of the present invention.

[0236] See also Figure 3 , Figure 3 This is a scanning electron microscope photograph of the molecular sieve prepared in the comparative example of the present invention.

[0237] from Figure 1 It can be seen from the XRD graph in that comparative example 1 is a pure MFI phase, and this is used as a comparative example. Examples 1-6 all have FER phase and MFI phase, and from Example 1 to Example 6, as the amount of sodium hydroxide introduced into the synthesis formula decreases, the FER characteristic peak in the XRD spectrum becomes more obvious, which means that the FER ratio in the FER-MFI eutectic increases.

[0238] from Figure 2 and 3 It can be seen from the SEM photo in that the molecular sieve synthesized in Comparative Example 1 has only the MFI phase, which is used as a control. In Examples 1 to 6, as the amount of alkali introduced in the synthesis ratio decreases, the FER phase in the synthesized FER-MFI molecular sieve increases continuously, while the MFI phase decreases continuously, which is consistent with the XRD spectrum.

[0239] Referring to Tables 1 to 7, Tables 1 to 6 are respectively the XRD spectrum information of the molecular sieve powders prepared in Examples 1 to 6 of the present invention, and Table 7 is the XRD spectrum information of the molecular sieve powder prepared in Comparative Example 1 of the present invention.

[0240] Table 1

[0241]

[0242] Table 2

[0243]

[0244] Table 3

[0245]

[0246] Table 4

[0247]

[0248]

[0249] Table 5

[0250]

[0251] Table 6

[0252]

[0253] Table 7

[0254]

[0255]

[0256] It is calculated from the XRD spectra information in Tables 1 to 6 that the mass content of the MFI phase is 80% to 98%.

[0257] The performance of the catalysts prepared in the examples of the present invention and the comparative examples was tested.

[0258] Catalytic evaluation test of fixed fluidized bed reactor

[0259] The test method is as follows:

[0260] Prepare 200g of catalyst and add it to the fixed fluidized bed reactor, set the system temperature to 630℃, nitrogen flow rate to 200mL / min, and water flow rate to 6g / min. After nitrogen fluidization and heating, the oil pump refluxes for 1min, feeds 20g of raw oil, reacts for 8min, strips for 20min, heats to 750℃, regenerates for 120min, and regeneration ends.

[0261] After the reaction is finished, record the amount of water, oil and gas inflow, take refinery gas for analysis and collect liquid products.

[0262] See Table 8, which shows the physical properties of the feedstock oil in Example 7 of the present invention.

[0263] Table 8

[0264]

[0265]

[0266] Statistics were performed on the catalytic cracking process in the examples.

[0267] See Table 9, which shows the physical properties and catalytic performance of the samples in Example 7 of the present invention.

[0268] Table 9

[0269]

[0270] As can be seen from Table 9, compared with the molecular sieve comparative example 1 with only the MFI phase, the diene yields of Examples 1 to 6 with the FER-MFI eutectic molecular sieve are all higher than those of comparative example 1. This is because the FER phase has a smaller pore structure, which makes it more selective for ethylene and propylene, and thus can obtain a higher diene yield. Moreover, as the proportion of the FER phase in the FER-MFI eutectic increases, the diene yield increases. While improving the selectivity, the present invention also notes that the introduction of the FER phase does not reduce the conversion rate of the reaction. Although the pore structure of the FER phase is small, which is not conducive to the entry of light hydrocarbon macromolecules into the pores for cracking, the FER-MFI eutectic synthesized by the present invention grows and connects together on a certain crystal plane. This allows the reactant molecules to directly enter the FER phase pores after the MFI phase pores react, while the larger molecules that cannot enter the FER phase pores will continue to enter the pores of the adjacent MFI phases to continue the reaction until they can enter the FER phase pores. In addition, it can be seen from the XRD spectrum of the present invention that, compared with a large amount of MFI phase, the FER phase only occupies a very small part, which can be seen from the diffraction peak height. This may be the reason why the FER-MFI eutectic molecular sieve prepared by the present invention can improve the reaction selectivity while maintaining the conversion rate.

[0271] The above is a detailed introduction to the preparation method and application of a eutectic FER-MFI molecular sieve provided by the present invention. Specific examples are used in this article to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method and its core ideas of the present invention, including the best mode, and also enables any technician in the field to practice the present invention, including the manufacture and use of any device or system, and the implementation of any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in several ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements that are not different from the text of the claims, or if they include equivalent structural elements that are not substantially different from the text of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. A method for preparing a FER-MFI molecular sieve, characterized in that: The following steps are involved: 1) mixing an aluminum source, a silicon source, a diamine-modified seed crystal, an alkaline substance and water to obtain a gel; 2) crystallizing the gel obtained in the above step and then calcining it to obtain a molecular sieve solid; 3) The molecular sieve solid obtained in the above step is subjected to ion exchange with ammonium salt and then calcined again to obtain the FER-MFI molecular sieve.

2. The preparation method according to claim 1, characterized in that: The diamine includes a C6-C10 long-chain diamine; The C6-C10 long-chain diamine includes one or more of hexamethylenediamine, heptamethylenediamine, octanediamine and nonamethylenediamine; The preparation steps of the diamine-modified seed crystals include: mixing the seed crystals with diamine and then performing amine treatment to obtain the diamine-modified seed crystals; The temperature of the amine treatment is 80 to 120°C; The amine treatment time is 8 to 12 hours; The molar ratio of the seed crystal to the diamine is (1-2): (5-10); The seed crystals are MFI phase seed crystals.

3. The preparation method according to claim 1, characterized in that: The aluminum source is one or more of aluminum hydroxide, sodium aluminate and pseudo-boehmite; The silicon source is one or more of silica gel, sodium silicate and silica sol; The silicon source and the aluminum source, calculated as SiO2 and Al2O3, have a molar ratio of (2-3): (0.1-0.2); The alkaline substance is one or more of an organic base and an inorganic base; The organic base includes one or more of tetrapropylammonium hydroxide, tetraethylammonium hydroxide, triethylamine and n-butylamine; The inorganic base includes one or more of potassium hydroxide, sodium hydroxide, sodium carbonate and sodium bicarbonate.

4. The preparation method according to claim 1, characterized in that: The aluminum source and the alkaline substance, calculated as Al and OH radical, have a molar ratio of (1-2): (0.1-1.5); The aluminum source is calculated as Al, and the molar ratio of the aluminum source to water is (1-2): (100-200); The mass ratio of the diamine modified seed crystal to the silicon source and the aluminum source, calculated as SiO2 and Al2O3, of the seed crystal to the total mass of SiO2+Al2O3 is (0.05-5):100; The step 1) specifically comprises the following steps: 11) mixing an aluminum source, an alkaline substance and water to obtain a solution; 12) continuing to mix the solution obtained in the above step with a silicon source to obtain a first gel; 13) The first gel obtained in the above step and the diamine-modified seed crystals are mixed again to obtain a gel.

5. The preparation method according to claim 1, characterized in that: The seed crystals are ZSM-5 molecular sieve seed crystals and / or S-1 molecular sieve seed crystals; The crystallization further includes a washing and / or drying step; The crystallization temperature is 160-180°C; The crystallization time is 24 to 72 hours; The calcination temperature is 500-700°C; The calcination time is 3 to 5 hours.

6. The preparation method according to claim 1, characterized in that: The ammonium salt is one or more of ammonium chloride, ammonium nitrate and ammonium acetate; The mass ratio of the ammonium salt to the molecular sieve solid is 1:(4-10); The re-calcination temperature is 500-700°C; The re-calcination time is 3 to 5 hours.

7. The preparation method according to claim 1, characterized in that: The FER-MFI molecular sieve is a eutectic-grown FER-MFI molecular sieve; The FER-MFI molecular sieve has a composite crystal structure of FER and MFI; The FER-MFI molecular sieve has a composite structure of FER micro-nano sheets and MFI nano-blocks; The FER micro-nanosheet has a radial dimension of 0.5 to 2 μm and a thickness of 20 to 60 nm; The particle size of the MFI nanoblock is 50-100nm*60-200nm; In the FER-MFI molecular sieve, the mass content of the MFI phase is 80% to 98%.

8. Use of the FER-MFI molecular sieve prepared by the preparation method according to any one of claims 1 to 7 in the field of light hydrocarbon cracking.

9. The use according to claim 8, characterized in that: The applications include the use of FER-MFI molecular sieve as a catalyst in the cracking process of light hydrocarbons; The application is specifically the application of the FER-MFI molecular sieve active component, kaolin and a binder combined as a composite catalyst; In the composite catalyst, the mass content of the FER-MFI molecular sieve active component is 30% to 50%; In the composite catalyst, the mass content of kaolin is 20% to 40%.

10. The use according to claim 9, characterized in that: The composite catalyst is specifically obtained by mixing, ball milling and molding the FER-MFI molecular sieve active component, kaolin and a binder; The binder includes one or more of alumina sol, silica sol, acidified pseudo-boehmite, water glass and aluminum phosphate; The light hydrocarbon raw material for cracking light hydrocarbons includes one or more of C5-C8 alkanes, olefins and aromatics; The reaction device of the light hydrocarbon cracking process includes a fixed fluidized bed reactor.

Citation Information

Patent Citations

  • Preparation method for ZSM-35 / ZSM-5 eutectic molecular sieve catalyst and application

    CN110756220A