Method for synthesizing high-silicon Cu-LTA molecular sieve in one step and application of high-silicon Cu-LTA molecular sieve

By synthesising high-silicon Cu-LTA molecular sieve catalysts in one step, the problem of insufficient hydrothermal stability of catalysts at high temperatures in the prior art is solved, and low-cost and efficient NH3-SCR activity and high-temperature hydrothermal stability are achieved. It is suitable for heavy-duty diesel NOx removal of Cheguo VI emission standards.

CN118929689APending Publication Date: 2024-11-12江西中科鸿虔新材料有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410980186.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to maintain the hydrothermal stability of NH3-SCR catalysts at high temperatures, especially when meeting the VI emission standards of heavy-duty diesel vehicles, the phase transformation of the carrier TiO2 of the V-based catalyst leads to the loss of the active component V2O5, and The catalyst preparation method is complex and costly.

Method used

Cu with excellent NH3-SCR activity and high temperature hydrothermal stability were prepared by mixing mother liquor, distilled water, adding HF aging, gel molding and rotary crystallization. -LTA molecular sieve catalyst.

Benefits of technology

A low-cost and efficient catalyst synthesis has been achieved. Cu-LTA molecular sieve maintains 90% NO conversion and 95% nitrogen selectivity at 250-550°C, and has good hydrothermal stability, which simplifies the preparation process and reduces the Post-processing cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929689A_ABST
    Figure CN118929689A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of catalysis, in particular to a method for synthesizing a high-silicon Cu-LTA molecular sieve in one step and application of the high-silicon Cu-LTA molecular sieve. According to the method for one-step synthesis of the high-silicon Cu-LTA molecular sieve, an active component Cu is subjected to one-step hydrothermal synthesis to form a Cu-LTA type molecular sieve catalyst with a high silica-alumina ratio, and the Cu-LTA type molecular sieve catalyst is applied to an NH3-SCR reaction; the LTA molecular sieve catalyst is synthesized through a dry gel hydrothermal method, catalyst samples with different silica-alumina ratios can be synthesized through the one-step synthesis method, an LTA molecular sieve with the high silica-alumina ratio of Si / Al = (9-30) can also be synthesized, and the content of the active component Cu ranges from 1.0 wt% to 4.0 wt% according to the difference of the silica-alumina ratios. According to the method for synthesizing the high-silicon Cu-LTA molecular sieve in one step and the application of the high-silicon Cu-LTA molecular sieve, one-step synthesis of the Cu-LTA molecular sieve with the high silica-alumina ratio is achieved, the molecular sieve catalyst has the advantages of being low in cost and efficient in synthesis, and the finally obtained product catalyst has efficient NH3-SCR catalytic activity and excellent high-temperature hydrothermal stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building decoration, and in particular to a method for synthesizing a high-silicon Cu-LTA molecular sieve in one step and application thereof. Background Art

[0002] Nitrogen oxides (NO x ) is an important precursor pollutant for haze and ozone pollution. Haze and ozone have serious negative impacts on the ecological environment. In addition, NO is also a blood poison, and its ability to bind to hemoglobin is stronger than that of CO. 2 It has a strong irritating effect on the respiratory tract. When inhaled into the human body, it can cause acute and chronic complications such as pulmonary edema, pneumothorax, and neurasthenia syndrome. At present, mobile sources have become the main source of NO in my country. x The main source of anthropogenic emissions is NO, which needs to be controlled urgently. x Accounting for mobile sources NO x 55.9% of total emissions, of which nearly 90% are NO x Emissions come from diesel vehicles; therefore, diesel vehicle exhaust NO x Emission control is crucial to control NO x The main source of emissions is NH 3 Selective Catalytic Reduction of NO x (NH 3 -SCR) technology, the core of which is NH 3 - Research and development of SCR catalysts; my country's National VI emission standards for heavy-duty diesel vehicles have been fully implemented. In order to meet the National VI emission standards for heavy-duty diesel vehicles, particulate filters (DPF) and SCR are used for PM and NO respectively in the post-treatment system. x In order to remove PM, after a certain amount of PM has accumulated, the DPF needs to be actively regenerated, which will expose the rear SCR catalyst to a high temperature and high humidity environment.

[0003] Therefore, under the current National VI emission standards and the National VII standards that may be implemented in the future, it is urgent to design and synthesize a NO x Catalytically active and hydrothermally stable catalysts, commonly used in NH 3 -SCR catalysts include metal oxide catalysts represented by V-based catalysts, Ce-based catalysts, Mn-based catalysts and Fe-based catalysts, and molecular sieve catalysts represented by SSZ-13 small-pore molecular sieves, ZSM-5 medium-pore molecular sieves and beta large-pore molecular sieves. V-based catalysts are low-priced, have high catalytic activity and excellent sulfur resistance, and are widely used in diesel vehicles that meet the National IV and National V standards in my country. x However, NH meets the National VI standard for diesel vehicles in my country. 3-SCR catalysts face more severe challenges and need to have good high-temperature hydrothermal stability; the carrier TiO2 of V-based catalysts at high temperatures 2 A phase transition will occur, resulting in the active component V 2 O 5 loss, in addition V 2 O 5 The volatilization of Cu also affects human health. To this end, researchers have developed many types of Cu-based small-pore molecular sieve catalysts, which have a wide temperature activity window, high N 2 Its selectivity and high hydrothermal stability make it the catalyst of choice for aftertreatment of diesel vehicles that meet the National VI standard.

[0004] The catalytic performance of a catalyst is mainly determined by its chemical composition and structure. The ingredients and dosage of the catalysts may be exactly the same, but due to different preparation methods, there may still be huge differences in the catalytic performance of the catalysts obtained. These properties of the catalyst are determined by the chemical composition and chemical and physical structure of the catalyst, which in turn depends on the composition, content, preparation method and pretreatment of the catalyst. In addition, the synthesis of the catalyst for industrial production also needs to consider whether the synthesis steps are simple and whether they comply with green production. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a one-step method for synthesizing a Cu-LTA molecular sieve with a high silicon-to-aluminum ratio. The Cu-LTA molecular sieve preparation method provided by the present invention realizes the low-cost and efficient synthesis of the Cu-LTA molecular sieve catalyst, and the final product has excellent NH3-SCR activity and high-temperature hydrothermal stability.

[0006] A one-step method for synthesizing high-silicon Cu-LTA molecular sieves of the present invention comprises the following steps:

[0007] Step 1: Mix the mother liquor, mix the silicon source, the aluminum source and the template agent in water for reaction, the template agent used is tetramethylammonium hydroxide template agent (TMAOH) and benzimidazole template agent (12DM3(4MB)1OH), and obtain the mixed mother liquor of Cu-LTA molecular sieve in one step;

[0008] Step 2, distilling water from the mother liquor, heating the obtained mixed mother liquor, and evaporating all ethanol and water generated by hydrolysis under continuous stirring to obtain a sol product;

[0009] Step 3, adding HF for aging, adding hydrofluoric acid (HF) to the obtained sol product, stirring evenly, to obtain a solid crude product;

[0010] Step 4: gel forming, adding the ground copper source to the obtained solid crude product to obtain the final gel, and then rotating the final gel for crystallization, filtering, washing, drying and calcining to obtain the Cu-LTA molecular sieve product.

[0011] Preferably, the silicon source and the aluminum source are SiO 2 and Al 2 O 3 The molar ratio of each raw material added in the synthesis of Cu-LTA molecular sieve is as follows: 12DM3(4MB)1OH:TMAOH:HF:SiO 2 :Al 2 O 3 :H 2 O=0.50:x:0.50:1.00:y:5.00, wherein x and y change according to the different Si / Al ratios of the synthesized Cu-LTA molecular sieve to obtain Cu-LTA molecular sieves with different silicon-aluminum ratios.

[0012] Preferably, the added molar ratio x of TMAOH is 0.01-0.7.

[0013] Preferably, Al 2 O 3 The added molar ratio y is 0.001-0.08.

[0014] Preferably, the benzimidazole templates used include hydroxyl type 1, 2-dimethyl 3-(4-methylbenzyl) imidazole (12DM3(4MB)1OH) and hydroxyl type 1, 2-dimethyl 3-(2-fluorobenzyl) imidazole (12DM3(2FB)1OH); the above-mentioned benzimidazole organic templates are used as templates for the crystallization reaction. Such organic substances all contain a cyclic structure and have a moderate molecular size, which play a structural guiding and filling role in the synthesis process of Cu-LTA molecular sieves. Moreover, such organic substances are charged in aqueous solution and play a charge filling role in the synthesis process of Cu-LTA molecular sieves.

[0015] Preferably, the hydroxyl-type 1,2-dimethyl 3-(4-methylbenzyl) imidazole (12DM3(4MB)1OH) benzimidazole template is prepared by the following method: an organic template precursor, 1,2-dimethyl imidazole, α-chloro-p-xylene and a solvent are mixed, reacted, separated, and ion-exchanged to obtain the hydroxyl-type organic template.

[0016] Preferably, the organic template precursor is subjected to a solvent mixing reaction, the solvent used is chloroform, and the mixing reaction time is 48 hours.

[0017] Preferably, the separation method of the organic template after the reaction includes suction filtration, centrifugation, rotary evaporation and recrystallization, and the recrystallization solvent is selected from methanol and ether.

[0018] Preferably, the ion exchange method comprises dispersing the recrystallized product in water, and then performing ion exchange with a hydroxide type cationic resin; the ion exchange is performed twice, each time for 24 hours.

[0019] Preferably, the silicon source includes tetraethyl orthosilicate and silica sol.

[0020] Preferably, the aluminum source includes aluminum hydroxide, pseudo-boehmite, aluminum sulfate.

[0021] Preferably, the copper source includes copper hydroxide, copper nitrate pentahydrate, copper acetylacetonate, basic copper carbonate.

[0022] The invention discloses an application of a one-step synthesis of high-silicon Cu-LTA molecular sieve, wherein the Cu-LTA molecular sieve prepared by the above one-step synthesis of high-silicon Cu-LTA molecular sieve is applied to NH 3 -In the catalytic reduction reaction of SCR, a NO conversion rate of 90% is achieved at 250-550°C, while maintaining a nitrogen selectivity of 95%.

[0023] Beneficial effects of the present invention: the one-step synthesis method of Cu-LTA described in the present invention adopts the dry gel method in the solvothermal method. The synthesis yield of this method is much higher than that of the ordinary solvothermal method, and the dry gel method is very compatible with the one-step synthesis method of copper-based molecular sieves. The added copper metal can more easily enter the appropriate reaction site, and it is easier to control the content of the copper source required to be added to the gel. Therefore, it is not necessary to perform copper reduction post-treatment on the molecular sieve. In addition, less synthetic waste liquid will be generated in the subsequent suction filtration and washing steps. This method solves the problems of high post-treatment cost and generation of pollutants, and at the same time eliminates the process of loading Cu on the LTA molecular sieve, further simplifying the preparation method;

[0024] The Cu-LTA molecular sieve of the present invention is a transition metal-based catalyst with a high-silicon LTA molecular sieve as a carrier, which has an LTA configuration, is a three-dimensional pore molecular sieve with four-membered rings, six-membered rings and eight-membered rings as basic components, and has three cage structures of different sizes, namely, LTA cages, SOD cages and Dr4 cages. Its specific pore structure determines that it has good application prospects in the field of NH3-SCR.

[0025] The present invention synthesizes Cu-LTA molecular sieves with different silicon-aluminum ratios by controlling the ratio of raw silicon and aluminum sources, and can have a very wide crystallization window under the raw material ratio described in the invention, can synthesize Cu-LTA molecular sieves with different silicon-aluminum ratios at different crystallization temperatures and times, and the Cu-LTA molecular sieve prepared by the method has very excellent hydrothermal stability;

[0026] The Cu-LTA molecular sieve preparation method provided by the present invention realizes the low-cost and efficient synthesis of the Cu-LTA molecular sieve catalyst, and the finally obtained product has excellent NH3-SCR activity and high-temperature hydrothermal stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is the XRD pattern of the Cu-LTA molecular sieve prepared in Example 1 of the present invention;

[0028] Figure 2 This is the first SEM image of the Cu-LTA molecular sieve prepared in Example 1 of the present invention;

[0029] Figure 3 is a second SEM image of the Cu-LTA molecular sieve prepared in Example 1 of the present invention;

[0030] Figure 4 Graph showing the NO conversion rates of Examples 1-4 of the present invention. DETAILED DESCRIPTION

[0031] Hereinafter, embodiments of the present invention will be described with reference to the drawings.

[0032] The preparation of the benzimidazole template comprises the following steps:

[0033] Step 1: Mix 0.10 mol 1,2-dimethylimidazole and 0.10 mol 4-Methylbenzylchloride (α-Chloro-p-xylene), stir continuously at room temperature for 48 h to obtain a white suspension, transfer the suspension to a rotary evaporator, evaporate under reduced pressure at 303 K for 0.5 h until the suspension becomes a white solid powder, raise the temperature to 333 K, and continue to evaporate under reduced pressure until a white powder is obtained. After complete drying, the white powder was dissolved in methanol, and 400 ml of ether was added under vigorous stirring for recrystallization. The product was filtered and rinsed three times with 100 ml of ether (or ethyl acetate). After evaporation under reduced pressure at 303 K for 30 min, it was further evaporated under reduced pressure at 363 K until complete drying. The white solid product obtained at this time was 1,2-Dimethyl-3-(4-methylbenzyl)imidazoliumchloride (12DM3(4MB)ICl), referred to as 12DM3(4MB)ICl.

[0034] Step 2: Dissolve 12DM3(4MB)ICl solid powder in deionized water, add appropriate amount of Amberlite IRN-78 anion exchange resin, and stir continuously at room temperature for 48 hours to obtain Cl - Completely exchanged to OH -, the mixed solution was filtered, the anion exchange resin was recovered and the liquid product was collected to obtain a 12DM3(4MB)IOH aqueous solution, and the solution was evaporated and concentrated under a 353K environment to obtain a 12DM3(4MB)IOH aqueous solution of appropriate concentration, which is a benzimidazole template (12DM3(4MB)1OH).

[0035] Step 3: Use phenolphthalein as an indicator and titrate the product solution with 0.01 mol / L dilute hydrochloric acid to determine the actual concentration of 12DM3(4MB)IOH.

[0036] Example 1

[0037] The preparation method of Cu-LTA molecular sieve in this embodiment is as follows:

[0038] First, mix the mother liquor and add 0.1927gAl(OH) 3 Dissolve in an appropriate amount (depending on the concentration) of 12DM3 (4MB) IOH aqueous solution, stir continuously for 1 hour to fully dissolve it, then add 0.348g TMAOH, continue stirring for 3 hours, add 5.6624g Tetraethylorthosilicate (TEOS) to the above mixture, stir vigorously for 16 hours to fully hydrolyze TEOS, and allow TEOS to convert Al(OH) 3 Completely converted to Al 2 O 3 , and obtain the mixed mother liquor of Cu-LTA molecular sieve in one step.

[0039] Then, the mother liquor was evaporated, and the obtained mixed mother liquor was heated to 343K. All ethanol and an appropriate amount of water generated by hydrolysis were evaporated under continuous stirring to make the water content of the target product meet the requirements of the sol (12DM3(4MB)1OH:TMAOH:HF:SiO 2 :Al 2 O 3 :H 2 O=0.50:0.05:0.50:1.00:0.033:5.00) to obtain a sol product.

[0040] Then, HF was added for aging, and the obtained sol product was transferred to a fume hood. A proper amount of hydrofluoric acid (HF) was added using a pipette and stirred evenly to obtain a solid crude product.

[0041] Finally, the gel was formed and 0.054 g of Cu(OH) 2After the solid is ground, it is added to the solid crude product, which is then transferred to a hydrothermal kettle, sealed and placed in an oven at 448K, and crystallized for 24 hours under continuous rotation (appropriately shortened or extended according to actual conditions). The hydrothermal synthesis product is then taken out and placed in a 500mL beaker, 300mL of deionized water is added, stirred evenly and allowed to stand for 3 hours, then filtered and washed with a large amount of deionized water, the powdered solid product is collected, and after drying under ventilation conditions for 12 hours, the sample solid powder is placed in a muffle furnace and calcined at 1173K at a heating rate of 1°C / min for 8 hours to completely remove the residual OSDA to obtain a Cu-LTA sample.

[0042] The mass percentage of Cu element in the Cu-LTA molecular sieve obtained in this example is 2.2wt%, and the Si / Al (silicon-aluminum ratio) is 11, and it is named Cu2.2-LTA-11.

[0043] The X-ray diffraction curve of the Cu2.2-LTA-11 molecular sieve prepared in this example is as follows: Figure 1 As shown in the figure, it can be seen that the product prepared in this example is a Cu2.2-LTA-11 molecular sieve with LTA configuration, and its diffraction peak positions are all standard characteristic peaks of LTA configuration molecular sieves. The SEM photo of this example is shown in Figure 2 and Figure 3 As shown, it is roughly in the shape of a cube with a particle size of 3 μm.

[0044] In order to verify the hydrothermal stability of the Cu2.2-LTA-11 molecular sieve described in this application, the prepared Cu2.2-LTA-11 molecular sieve was subjected to hydrothermal aging treatment at 850°C, 900°C, and 950°C for 16 hours, and then the removal rate of nitrogen oxides and the selectivity for nitrogen of the Cu2.2-LTA-11 molecular sieve after hydrothermal aging were tested.

[0045] Example 2

[0046] The difference between this embodiment and embodiment 1 is that the added Al(OH) 3 The amount was changed to 0.2356 g, and the other conditions were exactly the same as those in Example 1.

[0047] The mass percentage of Cu element in the Cu-LTA molecular sieve obtained in this example is 2.2%, and the silicon-aluminum ratio is 9, and it is named Cu2.2-LTA-9.

[0048] Example 3

[0049] The difference between this embodiment and embodiment 1 is that the added Al(OH) 3 The amount was changed to 0.1325 g, and the other conditions were exactly the same as those in Example 1.

[0050] The mass percentage of Cu element in the Cu-LTA molecular sieve obtained in this example is 2.2%, and the silicon-aluminum ratio is 16, and it is named Cu2.2-LTA-16.

[0051] Example 4

[0052] The difference between this embodiment and embodiment 1 is that the added Al(OH) 3 The amount was changed to 0.0922 g, and the other conditions were exactly the same as those in Example 1.

[0053] The Cu-LTA molecular sieve obtained in this example has a mass percentage of Cu element of 2.2% and a silicon-aluminum ratio of 23, and is named Cu2.2-LTA-23.

[0054] Example 5

[0055] The difference between this embodiment and embodiment 1 is that the added solid Cu(OH) 2 The amount was changed to 0.061 g, and the other conditions were exactly the same as those in Example 1.

[0056] The Cu-LTA molecular sieve obtained in this example has a mass percentage of Cu element of 2.5% and a silicon-aluminum ratio of 11, and is named Cu2.5-LTA-11.

[0057] Example 6

[0058] The difference between this embodiment and embodiment 1 is that the added solid Cu(OH) 2 The amount was changed to 0.044 g, and the other conditions were exactly the same as those in Example 1.

[0059] The mass percentage of Cu element in the Cu-LTA molecular sieve obtained in this example is 1.8%, and the silicon-aluminum ratio is 11, and it is named Cu1.8-LTA-11.

[0060] Example 7

[0061] The difference between this embodiment and embodiment 1 is that the added solid Cu(OH) 2 The amount was changed to 0.026 g, and the other conditions were exactly the same as those in Example 1.

[0062] The mass percentage of Cu element in the Cu-LTA molecular sieve obtained in this example is 1.0%, and the silicon-aluminum ratio is 11, and it is named Cu1.0-LTA-11.

[0063] Example 8

[0064] The difference between this embodiment and embodiment 1 is that the added solid Cu(OH) 2The amount was changed to 0.013 g, and the other conditions were exactly the same as those in Example 1.

[0065] The Cu-LTA molecular sieve obtained in this example has a mass percentage of Cu element of 0.5% and a silicon-aluminum ratio of 11, and is named Cu0.5-LTA-11.

[0066] Comparative Example 1

[0067] The difference between this comparative example and Example 1 is that the calcination temperature of the muffle furnace is changed to 873K.

[0068] Comparative Example 2

[0069] The difference between this comparative example and Example 1 is that the solid Cu(OH) 2 Use copper nitrate pentahydrate instead.

[0070] Performance Testing Methods

[0071] The Cu-LTA molecular sieve raw powder prepared in Example 1-4 was tableted, crushed, and sieved. A 40-60 mesh particle sample was placed in a quartz tube and used in a fixed bed reactor for nitrogen oxide removal rate and nitrogen selectivity testing. x ) removal rate test, the test conditions are as follows:

[0072] [NO]=[NH 3 ]=500ppm,[O 2 ]=[H 2 O]=5%,N 2 As the balance gas, the total flow rate of the reaction gas is 500mL / min, the reaction temperature range is 150℃-550℃, and the reaction stays at each temperature for 1h until the reaction is balanced. 3 , NO and reaction byproduct NO 2 、N 2 O concentrations were measured by infrared ThermoIS50; the catalyst dosage corresponded to a space velocity of 100,000 h -1 .

[0073] The test results are as follows Figure 4 As shown in the figure, the Cu-LTA molecular sieve prepared by the present invention has a high nitrogen oxide removal rate and nitrogen selectivity, and can be applied to NH 3 -In the catalytic reduction reaction of SCR, a NO conversion rate of 90% is achieved at 250-550°C, while maintaining a nitrogen selectivity of 95%.

[0074] The Cu-LTA molecular sieve raw powder prepared in Examples 1-8 and Comparative Examples 1-2 was tableted, crushed, and sieved. A 40-60 mesh particle sample was taken for hydrothermal aging test. The hydrothermal aging treatment conditions were: 10% H 2 O, air as carrier gas, air flow rate: 200mL / min, corresponding to the catalyst aging amount of 200mg, the hydrothermal aging treatment temperature is 850℃, 900℃, 950℃, and the hydrothermal aging treatment time is 16h.

[0075] The test results are shown in Table 1. According to the analysis results of hydrothermal aging T50 and T90 in Table 1, the Cu-LTA molecular sieve prepared by the present invention can maintain good thermal stability.

[0076] Table 1

[0077]

[0078] Those skilled in the art should understand that the above embodiments do not limit the present invention in any form, and any technical solutions obtained by equivalent replacement or equivalent transformation shall fall within the protection scope of the present invention.

Claims

1. A one-step method for synthesizing high-silicon Cu-LTA molecular sieves. It is characterized in that The following steps are included: Step 1, mixing mother liquor, mixing silicon source, aluminum source and template agent in water for reaction, the template agent used is tetramethylammonium hydroxide template agent and benzimidazole template agent, and obtaining the mixed mother liquor of Cu-LTA molecular sieve in one step; Step 2, distilling water from the mother liquor, heating the obtained mixed mother liquor, and evaporating all ethanol and water generated by hydrolysis under continuous stirring to obtain a sol product; Step 3, adding HF for aging, adding hydrofluoric acid to the obtained sol product, stirring evenly, to obtain a solid crude product; Step 4: gel forming, adding the ground copper source to the obtained solid crude product to obtain the final gel, and then successively subjecting the final gel to rotational crystallization, suction filtration, washing, drying and calcination to obtain the Cu-LTA molecular sieve product.

2. A one-step synthesis method of high silicon Cu-LTA molecular sieve according to claim 1, Its characteristics are: The silicon source and aluminum source were SiO 2 and Al 2 O 3 The molar ratio of each raw material added in the synthesis of Cu-LTA molecular sieve is as follows: 12DM3(4MB)1OH:TMAOH:HF:SiO 2 :Al 2 O 3 :H 2 O=0.50:x:0.50:1.00:y:5.00, wherein x and y change according to the different Si / Al ratios of the synthesized Cu-LTA molecular sieve to obtain Cu-LTA molecular sieves with different silicon-aluminum ratios.

3. A one-step synthesis method of high silicon Cu-LTA molecular sieve according to claim 2, Its characteristics are: The added molar ratio x of TMAOH is 0.01-0.

7.

4. A one-step synthesis method of high silicon Cu-LTA molecular sieve according to claim 2, Its characteristics are: Al 2 O 3 The added molar ratio y is 0.001-0.

08.

5. A one-step synthesis method of high-silicon Cu-LTA molecular sieve according to claim 1, Its characteristics are: The benzimidazole templates used include hydroxyl type 1, 2-dimethyl 3-(4-methylbenzyl) imidazole and hydroxyl type 1, 2-dimethyl 3-(2-fluorobenzyl) imidazole.

6. A one-step synthesis method of high-silicon Cu-LTA molecular sieve according to claim 5, Its characteristics are: The hydroxyl-type 1,2-dimethyl 3-(4-methylbenzyl) imidazole benzimidazole template used is prepared by the following method: an organic template precursor, 1,2-dimethyl imidazole, α-chloro-p-xylene and a solvent are mixed, reacted, separated, and ion-exchanged to obtain the hydroxyl-type organic template.

7. A one-step synthesis method of high-silicon Cu-LTA molecular sieve according to claim 1, Its characteristics are: Silicon sources include tetraethyl orthosilicate and silica sol.

8. A one-step synthesis method of high-silicon Cu-LTA molecular sieve according to claim 1, Its characteristics are: Aluminum sources include aluminum hydroxide, pseudo-boehmite, and aluminum sulfate.

9. A one-step synthesis method of high-silicon Cu-LTA molecular sieve according to claim 1, Its characteristics are: Copper sources include copper hydroxide, copper nitrate pentahydrate, copper acetylacetonate, and basic copper carbonate.

10. An application of a one-step synthesis of high-silicon Cu-LTA molecular sieve, which is an application of a Cu-LTA molecular sieve prepared by a one-step synthesis of high-silicon Cu-LTA molecular sieve according to any one of claims 1 to 9, Its characteristics are: Application of Cu-LTA molecular sieve in NH 3 -SCR catalytic reduction reaction.

Citation Information

Patent Citations

  • Cu / LTA catalyst and exhaust system, and manufacturing method of Cu / LTA catalyst

    CN108071450A

  • Preparation method and applications of high silicon Cu-LTA catalyst

    CN109985662A

  • Copper-based catalyst for ammonia selective catalytic reduction of NOx and preparation method of copper-based catalyst

    CN113070097A