Method for recovering residual lithium element in lithium precipitation filtrate in lithium sulfate lithium carbonate precipitation process
By adjusting the pH to 8-10 in the lithium sulfate precipitation of lithium carbonate process with acid, and using adsorbents to adsorb lithium ions, combined with acid washing to remove lithium and alkali treatment to remove impurities, the problem of insufficient lithium recovery in the lithium sulfate precipitation of lithium carbonate process is solved, and efficient recovery and production of high-purity by-products are achieved.
Patent Information
- Application Number
- CN202411206889.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-30
AI Technical Summary
In existing technologies, the residual lithium element in the filtrate of the lithium sulfate precipitation lithium carbonate process is not fully recovered, resulting in a decrease in lithium yield and low purity of by-products.
In the lithium sulfate precipitation process, the pH of the lithium precipitation filtrate is first adjusted to 8-10 by adding acid, and lithium ions are adsorbed by an adsorbent. Then, lithium is removed by acid washing and impurities are removed by alkali treatment. Finally, high-purity lithium chloride and high-purity anhydrous sodium sulfate are obtained by evaporation and crystallization.
The process achieved a high lithium recovery rate of over 90% in the lithium precipitation filtrate, and the high purity of the byproduct sodium sulfate and the reduction in sulfuric acid usage improved the overall economic efficiency and effectiveness of the process.
Smart Images

Figure CN118929704A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium element recovery, and in particular to a method for recovering residual lithium elements in a lithium precipitation filtrate in a lithium sulfate precipitation process for lithium carbonate. Background Art
[0002] With the rapid development of the global electric vehicle industry, the demand for lithium carbonate, a key raw material for preparing electric vehicle power batteries, has increased dramatically. As the demand for lithium carbonate increases, lithium carbonate and its preparation industry have received widespread attention in the industry.
[0003] The main source of lithium carbonate is to convert lithium ore, salt lakes and lithium from waste batteries into lithium sulfate through hydrometallurgical processes, and then convert lithium sulfate into lithium carbonate. The traditional process of converting lithium sulfate into lithium carbonate is as follows: Figure 1 As shown, lithium sulfate solution and excess sodium carbonate react to precipitate lithium carbonate and obtain crude lithium carbonate by filtration, and the filtrate is filtered to obtain solid sodium sulfate through freezing and crystallization. Since lithium carbonate has a solubility of 13.3g / L in aqueous solution and sodium carbonate and lithium sulfate cannot react completely, lithium ions remain in the filtrate after filtering lithium carbonate solid. The lithium ions remaining in the filtrate (sodium sulfate solution) will be partially separated out with sodium sulfate during the sodium sulfate cooling crystallization process to reduce the purity of the byproduct sodium sulfate, while reducing the yield of lithium. In addition, sodium ions and lithium ions will also remain in the mother liquor after freezing and crystallizing sodium sulfate, which will also reduce the yield of lithium.
[0004] The literature of the prior art mentions that the filtrate after cooling and crystallizing sodium sulfate is re-concentrated to make its lithium ion content reach about 1%, and a secondary lithium precipitation is performed to recover the residual lithium in the filtrate. However, this method still cannot fully recover the residual lithium element in the filtrate. Summary of the invention
[0005] In view of this, the present application provides a method for recovering the residual lithium element in the lithium precipitation filtrate in the lithium sulfate precipitation lithium carbonate process. The recovery method first adds sulfuric acid for pH control treatment before precipitating sodium sulfate in the traditional process, and then removes the lithium element in the filtrate by adsorption by an adsorbent, thereby reducing the lithium content in the filtrate. Sulfuric acid is then added to the sodium sulfate solution for purification to obtain a high-purity by-product sodium sulfate. At the same time, the adsorbent (i.e., the lithium-containing adsorbent) after adsorbing the lithium element is de-lithiated and impurities are removed to obtain high-purity lithium chloride, thereby realizing the recovery of the residual lithium element in the lithium precipitation filtrate in the lithium sulfate precipitation lithium carbonate process, and the recovery rate is as high as more than 90%. That is, the present process method takes into account the efficient recovery of lithium, the high purity of the by-product sodium sulfate, and the low total amount of sulfuric acid.
[0006] In the first aspect, the present application provides a method for recovering the residual lithium element in the lithium precipitation filtrate in the lithium sulfate precipitation lithium carbonate process. The lithium sulfate precipitation lithium carbonate process includes: reacting lithium sulfate solution with sodium hydroxide solution and sodium carbonate solution to precipitate lithium, filtering, and obtaining crude lithium carbonate and lithium precipitation filtrate. The recovery method includes at least the following steps: S100, adding acid to the lithium precipitation filtrate to adjust the pH to 8-10, and then adding an adsorbent to adsorb and extract lithium to obtain a sodium sulfate solution and a lithium-containing adsorbent, S200, acid-eluting the lithium-containing adsorbent to obtain a crude lithium chloride solution, S300, alkalizing and removing impurities from the crude lithium chloride solution, filtering, and obtaining a filtrate, and the filtrate contains Li + , Cl - and impurity cations, S400, subjecting the filtrate to a first evaporation crystallization to obtain crude lithium chloride crystals, the crude lithium chloride crystals are dissolved in an organic solvent, filtered, and Li + and Cl - The recovered liquid, S500, is subjected to a second evaporation crystallization to obtain high-purity lithium chloride, wherein in step S100, acid is added to the sodium sulfate solution, and high-purity anhydrous sodium sulfate is obtained by evaporation crystallization. In this application, the lithium precipitation filtrate obtained after lithium precipitation and filtration with lithium sulfate solution, sodium hydroxide solution, and sodium carbonate solution is first adjusted to a pH of 8 to 10 using acid. On the one hand, in an alkaline environment, the lithium extraction adsorbent has a better effect of adsorbing lithium ions. The lithium precipitation filtrate contains OH - 、CO3 2- , it is alkaline as a whole, but when the alkalinity is too strong, it will also damage the adsorbent and affect the lithium extraction effect. Therefore, adjusting the pH of the lithium precipitation filtrate to be in the range of 8 to 10 can obtain a better lithium adsorption effect while reducing the impact on the adsorbent; on the other hand, the adsorbent adsorbs Li + H + , causing the pH of the system to change towards the acidic direction, but because the system contains residual alkaline ions, such as CO3 2- , will be with H + The reaction keeps the system in a neutral or alkaline state, which is beneficial for the adsorbent to maintain a high efficiency during the entire adsorption and lithium extraction process; on the other hand, the adsorbent replaces H + , in an environment with a pH of 8-10, it is with CO3 2- The reaction not only weakens Li + With CO3 2- The interaction makes Li easier to be adsorbed in ionic state and reduces the CO3 2-The content of has the effect of removing impurities, so that a small amount of acid solution can be added to the sodium sulfate solution after lithium extraction to obtain high-purity sodium sulfate, and the total acid dosage is less, that is, while taking into account the high purity of sodium sulfate, the total acid dosage is reduced. Next, the present application adds an adsorbent to the lithium precipitation filtrate after adjusting the pH for adsorption and lithium extraction, and the adsorption and lithium extraction are completed to obtain a sodium sulfate solution and a lithium-containing adsorbent, and the sodium sulfate solution is acidified and purified and then evaporated and crystallized to obtain a by-product of high-purity anhydrous sodium sulfate. Finally, the lithium-containing adsorbent is de-lithiated to obtain high-purity lithium chloride, which realizes the efficient recovery of the residual lithium element in the lithium precipitation filtrate in the lithium sulfate precipitation lithium carbonate process, and takes into account the acquisition of high-purity anhydrous sodium sulfate.
[0007] In this process, CO3 in the lithium precipitation filtrate is used. 2- The H displaced by the adsorbent + , cooperate with each other, namely CO3 2- Consumption of H + , keeping the pH of the system always within the range of alkaline to neutral, ensuring the adsorption efficiency of the adsorbent; on the other hand, H + Also with CO3 2- The reaction removes it and generates CO2, which plays a role in removing impurities. The adsorption process mainly occurs in the following reactions, where R represents the lithium ion adsorbent:
[0008] 2R-H + +Li2CO3=2R-Li + +CO2+H2O
[0009] In some embodiments, the concentration of lithium ions in the lithium precipitation filtrate is 1.8 g / L to 2.0 g / L. The lithium ion concentration in the lithium precipitation filtrate is within the above range, which is more conducive to the full recovery of lithium elements. In this process, it is preferred to adjust the pH of the lithium precipitation filtrate by adding acid. When adjusting by adding acid, not only can the pH be 8 to 10, but also the concentration of lithium ions can be controlled within the range of 1.8 g / L to 2.0 g / L, that is, the concentration of lithium ions will not change too much when adding acid.
[0010] In some embodiments, in step S100, acidification includes: the acid added to the lithium precipitation filtrate includes a sulfuric acid solution, and preferably, the mass concentration of the sulfuric acid solution is 1% to 10%.
[0011] In some embodiments, in step S100, the adsorbent is a lithium ion adsorbent, and the lithium ion adsorbent Li + H +, which includes any one of manganese dioxide ion sieve, titanium oxide ion sieve, high-valent amorphous phosphate, hydrated SnO2, and amorphous Al(OH)3. Specifically, in some examples, the adsorbent is manganese dioxide ion sieve, and the lithium precipitation filtrate after pH adjustment flows through the manganese dioxide ion sieve at a flow rate of 3BV / h to 4BV / h to adsorb and extract lithium to obtain a lithium-containing adsorbent, wherein the manganese dioxide ion sieve is granular and has a bulk density of 70g / cm 3 Up to 75g / cm 3 . In this way, it is more conducive to the adsorption and lithium extraction of manganese dioxide ion sieve. In other examples, the adsorbent is titanium oxide ion sieve, and the lithium precipitation filtrate after pH adjustment flows through the titanium oxide ion sieve at a flow rate of 5BV / h to 7BV / h for adsorption and lithium extraction to obtain a lithium-containing adsorbent, wherein the titanium oxide ion sieve is in powder form, 90% of which has a particle size between 1μm and 3μm, and an average particle size of 1.6 to 1.8μm. In this way, it is more conducive to the adsorption and lithium extraction of titanium oxide ion sieve.
[0012] In some embodiments, in step S200, the acid-eluting lithium comprises: mixing a lithium-containing adsorbent and a hydrochloric acid solution to perform a lithium-elution reaction, wherein the concentration of the hydrochloric acid solution is in the range of 0.01 mol / L to 1 mol / L, and the adsorbent after lithium-elution is returned to step S100 to continue to adsorb and extract lithium. In the present application, the lithium-containing adsorbent is subjected to acid-eluting desorption with hydrochloric acid of a suitable concentration to obtain a crude lithium chloride solution, which comprises lithium chloride (Li in the lithium-containing adsorbent) + and H in hydrochloric acid + Replacement), manganese chloride (produced by adsorbent dissolution), etc. The concentration of the hydrochloric acid solution is within the above range to avoid increasing the dissolution rate of the adsorbent. The present application controls the dissolution rate within a suitable range, which is beneficial for obtaining high-purity lithium chloride with a high yield on the one hand, and can also save process costs, improve the effect and service life of the adsorbent, and is more conducive to large-scale industrial production on the other hand.
[0013] In some embodiments, in step S300, alkalization and impurity removal include: adding alkali to the crude lithium chloride solution to adjust the pH to 7-8. Preferably, the alkali used in the alkalization and impurity removal includes at least one of sodium hydroxide solution, lithium hydroxide solution, and sodium carbonate solution. More preferably, the alkali used in the alkalization and impurity removal includes a sodium hydroxide solution with a mass percentage of 20wt% to 25wt%. In the present application, the crude lithium chloride solution is adjusted to a pH of 7-8 by adding alkali, and after the reaction is completed, insoluble impurities such as manganese hydroxide (manganese chloride produced by the dissolution of the adsorbent is converted into manganese hydroxide under alkaline conditions) are filtered to obtain a filtrate, and the filtrate contains Li + , Cl - As well as impurity cations. This provides the possibility for subsequent purification to obtain high-purity lithium chloride. Impurity cations include cations in alkali solution, such as Na + wait.
[0014] In some embodiments, in step S400, the organic solvent is selected from anhydrous ethanol and / or anhydrous acetone. In the present application, the crude lithium chloride containing chloride salt is dissolved by adding a suitable organic solvent, which is more conducive to obtaining high-purity lithium chloride and improving its yield. After the dissolution is completed, the chloride salt is removed by filtering to obtain the lithium chloride containing only Li + and Cl - of recovery fluid.
[0015] In some embodiments, in step S500, the organic solvent obtained by subjecting the recovered liquid to a second evaporation crystallization and cooling is continuously returned to step S400 to dissolve the crude lithium chloride, wherein the temperature range of the second evaporation crystallization is 100° C. to 280° C. The present application regulates the temperature of the second evaporation crystallization within the above range, which is beneficial to obtaining high-purity lithium chloride on the one hand, and is also more conducive to the recycling of the organic solvent on the other hand, further reducing the process cost.
[0016] In some embodiments, in the lithium sulfate precipitation lithium carbonate process, the concentration of the lithium sulfate solution is 200g / L to 260g / L, the concentration of the sodium carbonate solution is 150g / L to 300g / L, and the molar ratio of sodium carbonate in the sodium carbonate solution to lithium sulfate in the lithium sulfate solution is 1.0 to 1.2.
[0017] In some embodiments, the conditions of the lithium precipitation reaction include: lithium precipitation temperature: 15°C to 98°C, reaction time: 0.2h to 3h. In this way, it is more conducive to obtaining a lithium precipitation filtrate with a suitable lithium ion concentration, and thus more conducive to the recovery of lithium elements. Preferably, the lithium precipitation temperature is 80°C to 90°C, and the reaction time is 0.2h to 0.5h.
[0018] The present application adds acid to the lithium precipitation filtrate after filtering out the crude lithium carbonate to adjust the pH to 8-10, and then adsorbs the lithium ions in the lithium precipitation filtrate with an adsorbent. According to the test, the concentration of lithium ions in the lithium precipitation filtrate can be reduced by about 600 times or more after adsorption by the adsorbent. The lithium-containing adsorbent is acid-eluted with hydrochloric acid to obtain a lithium-containing washing liquid (i.e., a crude lithium chloride solution), and the lithium-containing washing liquid is added with alkali to remove impurities (such as manganese ions) generated by the dissolution of the adsorbent, filtered, and the filtrate is evaporated and crystallized to obtain crude lithium chloride crystals (containing sodium chloride or potassium chloride). The crude lithium chloride crystals are dissolved and filtered with an organic solvent to separate the chloride salt insoluble matter (such as sodium chloride), and the organic solvent filtrate is evaporated and crystallized to obtain high-purity lithium chloride, thereby achieving full recovery of residual lithium elements in the filtrate.
[0019] In this application, by utilizing the CO3 in the lithium precipitation filtrate 2- With H in the adsorbent + The interaction not only realizes the Li + More importantly, the adsorption process can be kept in a neutral or alkaline environment, maintaining the high adsorption capacity of the adsorbent and also removing the impurity CO32- Removal is beneficial to obtaining high-purity sodium sulfate by-product. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0021] Figure 1 This is a schematic diagram of the traditional process flow for converting lithium sulfate into lithium carbonate;
[0022] Figure 2 The present invention is a schematic diagram of the process flow of a method for recovering residual lithium in a lithium carbonate precipitation process using lithium sulfate in the present application. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0024] Method for recovering residual lithium element in lithium precipitation filtrate in lithium sulfate precipitation lithium carbonate process
[0025] The lithium precipitation filtrate is obtained by the following process: lithium sulfate solution is reacted with sodium hydroxide solution and sodium carbonate solution to precipitate lithium, and filtered to obtain crude lithium carbonate and lithium precipitation filtrate, wherein the specific operation can refer to the conventional steps of the prior art, or can be obtained by the method disclosed in this application.
[0026] See also Figure 2 , the recovery method mainly includes the following steps:
[0027] S100, adding acid to the lithium precipitation filtrate to adjust the pH to 8-10, then adding an adsorbent to adsorb and extract lithium to obtain a sodium sulfate solution and a lithium-containing adsorbent, and the sodium sulfate solution is neutralized and purified by adding acid, and then evaporated and crystallized to obtain high-purity anhydrous sodium sulfate;
[0028] S200, removing lithium from the lithium-containing adsorbent by acid elution to obtain a crude lithium chloride solution;
[0029] S300, the crude lithium chloride solution is alkalized and impurities are removed, and filtered to obtain a filtrate, which contains Li + , Cl - and impurity cations;
[0030] S400, subjecting the filtrate to a first evaporation crystallization to obtain crude lithium chloride crystals, dissolving the crude lithium chloride crystals in an organic solvent, filtering, and obtaining a solid containing Li + and Cl - of recovery fluid;
[0031] S500, subjecting the recovered liquid to a second evaporation crystallization to obtain high-purity lithium chloride.
[0032] The conditions for the first evaporation crystallization and the second evaporation crystallization may be the same or different, but are preferably the same.
[0033] The present application firstly performs pH control treatment on the lithium precipitation filtrate after lithium precipitation and filtration of lithium sulfate solution, sodium hydroxide solution and sodium carbonate solution by adding acid, and then extracts lithium by adsorption of lithium by lithium adsorbent. In this way, the lithium ion concentration in the sodium sulfate solution is reduced by more than 600 times than the lithium ion concentration in the lithium precipitation filtrate, thereby improving the purity of the byproduct sodium sulfate. At the same time, the present application continues to alkalize and remove impurities from the lithium-containing washing liquid (crude lithium chloride solution) after the lithium-containing adsorbent is acid-eluted to obtain crude lithium chloride crystals, and then uses an organic solvent to dissolve and remove impurities from the crude lithium chloride crystals, and finally obtains high-purity lithium chloride by secondary evaporation and crystallization, thereby achieving full recovery of the residual lithium element in the lithium precipitation filtrate, and the recovery rate of the lithium element is as high as more than 90%.
[0034] In some embodiments, the concentration of lithium ions in the lithium precipitate filtrate is 1.8 g / L to 2.0 g / L. The concentration of lithium ions in the lithium precipitate filtrate is appropriately regulated, which is more conducive to the recovery of residual lithium elements in the lithium carbonate precipitate filtrate. Exemplarily, the concentration of lithium ions in the lithium precipitate filtrate is 1.8 g / L, 1.83 g / L, 1.85 g / L, 1.87 g / L, 1.89 g / L, 1.9 g / L, 1.91 g / L, 1.95 g / L, 1.98 g / L, 2.0 g / L or a value within the range of any two of these values.
[0035] In some embodiments, in step S100, adding acid to adjust the pH to 8-10 includes: adding sulfuric acid solution to the lithium precipitation filtrate to adjust the pH value to 8 to 10. Adding acid to adjust the pH to the above range is beneficial to improving the lithium absorption effect of the adsorbent on the one hand, and on the other hand, it can further improve the purity of sodium sulfate and maintain the high performance of the adsorbent. Exemplarily, sulfuric acid solution is added to the lithium precipitation filtrate to adjust the pH value to 8, 8.5, 9, 9.5, 10 or a value within the range composed of any two of these values.
[0036] In some embodiments, the mass concentration of the sulfuric acid solution is 1wt% to 10wt%. In this way, the residual lithium carbonate in the lithium precipitation filtrate is converted into lithium sulfate with high solubility, further improving the recovery rate of the lithium element. Exemplarily, the mass concentration of the sulfuric acid solution is 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 8wt%, 10wt% or a value within the range composed of any two of these values.
[0037] In some embodiments, in step S100, the adsorbent is a lithium ion adsorbent, which includes any one of manganese dioxide ion sieve, titanium oxide ion sieve, high-valent amorphous phosphate, hydrated SnO2, and amorphous Al(OH)3. Among them, manganese dioxide ion sieve is preferred as the lithium adsorbent because of its low price, good cycle performance, and large lithium adsorption capacity.
[0038] For example, the adsorbent is a manganese dioxide ion sieve, and the acidified lithium precipitation filtrate flows through the manganese dioxide ion sieve at a flow rate of 3BV / h to 4BV / h for adsorption and lithium extraction. The manganese dioxide ion sieve is granular and has a bulk density of 70g / cm 3 Up to 75g / cm 3 . Exemplarily, the flow rate of the acidified lithium precipitation filtrate through the manganese dioxide ion sieve is 3BV / h, 3.2BV / h, 3.3BV / h, 3.5BV / h, 3.6BV / h, 3.8BV / h, 4BV / h or a value in the range of any two of these values. Exemplarily, the bulk density of the manganese dioxide ion sieve is 70g / cm 3 、71g / cm 3 , 72g / cm 3 、73g / cm 3 , 74g / cm 3 , 75g / cm 3 Or a value within the range consisting of any two of these values.
[0039] Exemplarily, the adsorbent is titanium oxide ion sieve, and the acidified lithium precipitation filtrate flows through the titanium oxide ion sieve at a flow rate of 5BV / h to 7BV / h for adsorption and lithium extraction. The titanium oxide ion sieve is in powder form, and its 90% particle size is between 1μm and 3μm, and the average particle size is 1.6μm to 1.8μm. Exemplarily, the flow rate of the acidified lithium precipitation filtrate flowing through the titanium oxide ion sieve is 5BV / h, 5.3BV / h, 5.5BV / h, 5.8BV / h, 6BV / h, 6.5BV / h, 6.8BV / h, 7BV / h or a value in the range of any two of these values. Exemplarily, the 90% particle size of the titanium oxide ion sieve is 1μm, 1.3μm, 1.5μm, 1.8μm, 2μm, 2.5μm, 3μm or a value in the range of any two of these values. Illustratively, the average particle size of the titanium oxide ion sieve is 1.6 μm, 1.65 μm, 1.68 μm, 1.7 μm, 1.75 μm, 1.8 μm, or a value within a range consisting of any two of these values.
[0040] In some embodiments, in step S200, acid-eluting lithium includes: mixing a lithium-containing adsorbent and a hydrochloric acid solution to perform a lithium-removal reaction, the concentration range of the hydrochloric acid solution is 0.01 mol / L to 1 mol / L, and the adsorbent after lithium-removal is returned to step S100 to continue to adsorb and extract lithium. The present application uses a hydrochloric acid solution of a certain concentration to acid-elute lithium from the lithium-containing adsorbent, and the lithium-removal effect is good, and the obtained crude lithium chloride solution is more conducive to recovering lithium elements. Exemplarily, the concentration of the hydrochloric acid solution is 0.01 mol / L, 0.03 mol / L, 0.05 mol / L, 0.07 mol / L, 0.09 mol / L, 1 mol / L or a value within the range composed of any two of these values.
[0041] In some embodiments, in step S300, alkalization and impurity removal include: adding alkali to the crude lithium chloride solution to adjust the pH to 7-8. The purpose of adding alkali to adjust the pH to 7-8 is to neutralize the excess acid in the acid-eluted lithium and the impurities (such as manganese chloride) produced by the loss of the lithium-containing adsorbent in an acidic environment. In some examples, the alkali used in alkalization and impurity removal includes at least one of sodium hydroxide solution, lithium hydroxide solution, and sodium carbonate solution. In other examples, the alkali used in alkalization and impurity removal includes 20wt% to 25wt% sodium hydroxide solution. When the type of alkali and the pH value of the solution are appropriate, it is more conducive to obtaining high-purity lithium chloride with a high yield.
[0042] In some embodiments, in step S400, the organic solvent is selected from anhydrous ethanol and / or anhydrous acetone. Anhydrous ethanol and / or anhydrous acetone are more conducive to dissolving the chloride salt in the crude lithium chloride to obtain a lithium chloride containing only Li + and Cl - of recovery fluid.
[0043] In some embodiments, in step S500, the organic solvent obtained by the second evaporation crystallization of the recovered liquid is continuously returned to step S400 to dissolve the crude lithium chloride crystals, and the temperature range of the second evaporation crystallization is 100° C. to 280° C. Exemplarily, the temperature range of the second evaporation crystallization is 100° C., 130° C., 150° C., 180° C., 200° C., 220° C., 250° C., 260° C., 280° C., or a value within the range consisting of any two of these values.
[0044] In some embodiments, in the lithium sulfate precipitation lithium carbonate process, the concentration of the lithium sulfate solution is 200g / L to 260g / L, the concentration of the sodium hydroxide solution is 40g / L to 80g / L (about 4wt% to 8wt%), the concentration of the sodium carbonate solution is 150g / L to 300g / L, and the molar ratio of the sodium carbonate in the sodium carbonate solution to the lithium sulfate in the lithium sulfate solution is 1.0 to 1.2; and / or, the conditions for the lithium precipitation reaction include: lithium precipitation temperature: 15°C to 98°C, reaction time: 0.2h to 3h. Exemplarily, the concentration of the lithium sulfate solution is 200g / L, 210g / L, 220g / L, 230g / L, 240g / L, 245g / L, 250g / L, 260g / L or a value within the range composed of any two of these values. Exemplarily, the concentration of the sodium hydroxide solution is 40g / L, 45g / L, 50g / L, 55g / L, 60g / L, 65g / L, 70g / L, 75g / L, 80g / L, or a value in the range consisting of any two of these values. Exemplarily, the concentration of the sodium carbonate solution is 150g / L, 160g / L, 180g / L, 200g / L, 230g / L, 260g / L, 270g / L, 280g / L, 300g / L, or a value in the range consisting of any two of these values. Exemplarily, the ratio of the molar amount of sodium carbonate in the sodium carbonate solution to the molar amount of lithium sulfate in the lithium sulfate solution is 1.0, 1.05, 1.1, 1.13, 1.15, 1.18, 1.2, or a value in the range consisting of any two of these values.
[0045] The following are possible implementations
[0046] The main purpose of the present invention is to provide a method for recovering residual lithium in lithium precipitation mother liquor in a lithium sulfate precipitation process of lithium carbonate, aiming to solve the problem that the existing technical solutions cannot fully recover the residual lithium in the lithium precipitation filtrate.
[0047] To achieve the above object, the present invention provides a method for recovering residual lithium in lithium carbonate precipitation mother liquor in a lithium sulfate precipitation process, which comprises the following steps:
[0048] S1, the lithium sulfate solution is mixed with the sodium hydroxide solution and the sodium carbonate solution in sequence to perform a lithium precipitation reaction, and after the lithium precipitation reaction is completed, the crude lithium carbonate and the filtrate are filtered to obtain the crude lithium carbonate, and the crude lithium carbonate is washed to obtain the product high-purity lithium carbonate. Further, the lithium sulfate solution and the sodium hydroxide solution are first mixed, the pH of the solution after mixing is an alkaline environment, and then the sodium carbonate solution is added to perform a lithium precipitation reaction.
[0049] S2, adding sulfuric acid to the filtrate obtained in S1 to adjust the pH value. The pH value of the solution after adjustment is in the range of 8-10. The purpose of pH adjustment is to protect the molecular sieve from deterioration while providing a better molecular sieve adsorption environment. In addition, the hydrogen ions displaced by adsorption can react with carbonate ions in the solution to reduce the acid consumption.
[0050] S3, the filtrate after pH control of S2 is subjected to lithium adsorption and extraction by a lithium adsorbent, and a sodium sulfate solution and a lithium-containing adsorbent are obtained after the adsorption and extraction of lithium. The sodium sulfate solution is neutralized, purified, evaporated and crystallized to obtain a by-product of high-purity anhydrous sodium sulfate.
[0051] S4, adding hydrochloric acid solution to the lithium-containing adsorbent obtained in S3 to perform acid washing to remove lithium, and obtaining lithium adsorbent and crude lithium chloride solution after the acid washing, and the lithium adsorbent is returned to the S3 process for repeated use.
[0052] S5, adding a strong base to the crude lithium chloride solution obtained in S4 to adjust the pH range to 7-8, filtering to remove insoluble impurities such as manganese hydroxide after the reaction is completed to obtain a filtrate, and then performing a first evaporation crystallization to obtain crude lithium chloride crystals containing chloride salt.
[0053] S6, adding an organic solvent to dissolve the crude lithium chloride crystals (LiCl is easily soluble in ethanol, for example) obtained in S5, and filtering to remove impurity chloride salts to obtain a filtrate after the dissolution is completed.
[0054] S7, performing a second evaporation crystallization on the filtrate obtained in S6 to obtain an organic solvent and a by-product of high-purity lithium chloride, and the organic solvent is returned to S6 for recycling.
[0055] Furthermore, the lithium sulfate in the above step S1 can be obtained by smelting lithium ore, salt lakes and waste batteries, or can be commercially available, and its concentration range is 165-240 g / L. The pH range of the solution after adding the sodium hydroxide solution is 11-12. The concentration range of the sodium carbonate solution is 150-300 g / L, and the amount of sodium carbonate added is 1.0-1.2 times the molar amount of lithium sulfate, preferably 1.02-1.07 times.
[0056] Furthermore, in the above step S1, the lithium precipitation temperature is 15-98°C, preferably 80-95°C. The reduction of lithium carbonate solubility under high temperature conditions helps to increase the lithium carbonate yield. The reaction time can be 0.2-3h, preferably 0.4-0.6h.
[0057] Furthermore, in the above step S3, the lithium adsorbent can be selected from manganese dioxide ion sieve, titanium oxide ion sieve, high-valent amorphous phosphate, such as titanium phosphate, tin phosphate and zirconium phosphate, hydrated SnO2, amorphous Al(OH)3, etc. Among them, manganese dioxide ion sieve is preferred as the lithium adsorbent due to its low price, good cycle performance and high lithium adsorption capacity.
[0058] Furthermore, in the above step S3, the distillation and crystallization temperature of the sodium sulfate solution can range from 150°C to 300°C.
[0059] Furthermore, the concentration of hydrochloric acid used to elute lithium in the above step S4 is in the range of 0.01-1 mol / L, preferably in the range of 0.3-0.6 mol / L.
[0060] Furthermore, the purpose of adding alkali (such as Na2CO3) in the above step S5 to adjust the pH to 7-8 is to neutralize the excess acid in the acid washing and impurities generated by the loss of the precipitated lithium adsorbent.
[0061] Furthermore, the organic solvent used in step S6 is an alcohol organic solvent, which can be one or more mixed solvents such as methanol, ethanol, etc.
[0062] Furthermore, in step S7, the second evaporation crystallization temperature of lithium chloride can range from 100 to 280°C, preferably from 170 to 260°C.
[0063] Hereinafter, examples and comparative examples are given to more specifically illustrate the embodiments of the present application. Unless otherwise stated, the parts, percentages and ratios listed are all based on mass.
[0064] The manganese dioxide ion sieve used in the embodiment is an existing material, and its preparation method is briefly described below:
[0065] Li 1.6 Mn 1.6 After O4, PVC powder and KCl fine powder are evenly mixed, NN-dimethylformamide solvent is added, stirred until a colloid is formed, and dried at 80°C. The sample is crushed and soaked in water to dissolve all the KCl therein. After the sample is dried, a granular adsorbent precursor is obtained. Then, the granular ion sieve adsorbent is obtained by acid leaching to remove lithium, washing with water, and drying.
[0066] Example 1
[0067] To 1L of 220g / L lithium sulfate solution, 1.22g of 5% sodium hydroxide solution was added to adjust the pH of the solution to 11.2, and then 0.86L of 260g / L sodium carbonate solution was added. The mixture was reacted at 85°C for 0.5h. After the reaction was completed, crude lithium carbonate and the filtrate obtained by the reaction (lithium precipitation filtrate) were filtered. The crude lithium carbonate was washed three times with deionized water to obtain 129.58g of lithium carbonate with a purity of 99.57%.
[0068] 2.7 g of 5% sulfuric acid was added to the filtrate obtained by the reaction to adjust the pH value to 10. At this time, the lithium ion concentration was measured to be 1.910 g / L. The filtrate obtained after pH adjustment was passed through 580 g of manganese dioxide ion sieve at a flow rate of 3.5 BV / h for adsorption and lithium extraction. The manganese dioxide ion sieve was granular and consisted of Li 1.6 Mn 1.6 O4 and PVC organic resin bonding and pore-forming agent NN-dimethylformamide were prepared, Li 1.6 Mn 1.6 The mass ratio of O4 and organic resin PVC is about 7:2, and the bulk density is about 72g / cm 3 The sodium sulfate solution obtained by adsorption and extraction of lithium was tested, and its lithium content was reduced to 2 mg / L, which was about 950 times lower than the lithium ion content before adsorption (1.91 g / L). 32.98 g of 30% sulfuric acid was added to the sodium sulfate solution after adsorption, and then 298.81 g of high-purity sodium sulfate with a purity of 99.93% was obtained by evaporation and crystallization. The results are shown in Table 1.
[0069] The lithium adsorbent was delithiated with 1.78L of 0.5mol / L hydrochloric acid, and 64g of 25% sodium hydroxide solution was added to the delithiation solution (i.e., crude lithium chloride solution), and then filtered to remove impurities. After impurities were removed, the filtrate was evaporated and crystallized to obtain crude lithium chloride, and the crude lithium chloride was added to 30g of ethanol solution for dissolution. After the dissolution was completed, 20.7g of lithium chloride with a purity of 99.97% was obtained by filtration, evaporation and crystallization.
[0070] This time, 220g of lithium sulfate was added, which was equivalent to 27.79g of lithium equivalent, and 129.58g of lithium carbonate with a purity of 99.57% and a lithium equivalent of 24.24g were obtained. That is, the remaining lithium equivalent in the lithium carbonate filtrate (i.e., the lithium precipitation filtrate) was 3.55g, and after subsequent recovery, 20.7g of lithium chloride with a purity of 99.97% was generated, and the lithium equivalent was 3.39g. The recovery rate of residual lithium in the solution was Q1=3.39 / 3.55*100=95.5%.
[0071] Example 2
[0072] To 1L of 245g / L lithium sulfate solution, add 7.96g of 5% sodium hydroxide solution to adjust the pH of the solution to 12, then add 0.9L of 270g / L sodium carbonate solution, react at 85°C for 0.5h, filter after the reaction to obtain crude lithium carbonate and the filtrate obtained by the reaction (lithium precipitation filtrate), wash the crude lithium carbonate three times with deionized water to obtain 145.33g of lithium carbonate with a purity of 99.62%.
[0073] Add 22.91g of 10wt% sulfuric acid to the filtrate obtained by the reaction to adjust the pH to 8. At this time, the lithium ion concentration is measured to be 1.902g / L. The filtrate obtained after adjusting the pH flows through 115gH2TiO3 ion sieve at a flow rate of 6BV / h for adsorption and lithium extraction. The ion sieve used is powdered, 90% of the particle size is between 1-3μm, and the average particle size is about 1.8 microns. The sodium sulfate solution obtained after adsorption and lithium extraction was tested, and its lithium content dropped to 3mg / L, which is about 634 times lower than the lithium ion content before adsorption (1.902g / L). Add 21.85g of sulfuric acid with a concentration of 30% to the sodium sulfate solution after adsorption, and then evaporate and crystallize to obtain 326.87g of high-purity sodium sulfate with a purity of 99.91%. See Table 1 for the results.
[0074] The lithium adsorbent was delithiated with 1.25L of 0.5mol / L hydrochloric acid, and 61.27g of 25% sodium hydroxide solution was added to the delithiated solution (crude lithium chloride solution), and then filtered to remove impurities. After impurities were removed, the filtrate was evaporated and crystallized to obtain crude lithium chloride, and the crude lithium chloride was added to 40g of ethanol solution for dissolution. After the dissolution was completed, 21.2g of lithium chloride with a purity of 99.94% was obtained by filtration and evaporation and crystallization.
[0075] This time, 245g of lithium sulfate was added, which was equivalent to 30.95g of lithium equivalent, and 145.33g of lithium carbonate with a purity of 99.62% and a lithium equivalent of 27.20g were obtained. That is, the remaining lithium equivalent in the lithium carbonate filtrate (i.e., the lithium precipitation filtrate) was 3.75g, and after subsequent recovery, 21.2g of lithium chloride with a purity of 99.94% was generated, and the lithium equivalent was 3.47g. The recovery rate of residual lithium in the solution was Q1=3.47 / 3.75*100=92.5%.
[0076] Comparative Example 1 (no acid was added to adjust pH, and the obtained lithium precipitation filtrate was directly used for lithium extraction with an adsorbent)
[0077] To 1L of lithium sulfate solution with a concentration of 220g / L, 1.22g of 5% sodium hydroxide solution was added to adjust the pH of the solution to 11.2, and then 0.86L of sodium carbonate solution with a concentration of 260g / L was added, and the reaction was carried out at 85°C for 0.5h. After the reaction, the filtration operation was performed to obtain lithium carbonate and filtrate, and the lithium carbonate was washed three times with deionized water to obtain 130.46g of lithium carbonate with a purity of 99.28%. After the lithium precipitation test, the lithium ion concentration of the filtrate was 1.913g / L and the pH was 11.2. The filtrate was not adjusted in pH and directly passed through 580g of the same ion sieve as Example 1 at a flow rate of 3.5BV / h. The sodium sulfate solution obtained by adsorption and extraction of lithium was tested, and its lithium content was 58mg / L, which was only 32.98 times lower than the lithium ion content before adsorption. The adsorbed sodium sulfate solution was added with 33.38 g of 30% sulfuric acid, and then evaporated and crystallized to obtain 303.75 g of sodium sulfate with a purity of 98.28%.
[0078] In Example 1, the filtrate after lithium precipitation was pH adjusted and then subjected to ion sieve adsorption to extract lithium. After adsorption, the lithium ion content was greatly reduced by 950 times. In addition, the purity of sodium sulfate obtained by using sulfuric acid reached 99.93%. In Comparative Example 1, the filtrate after lithium precipitation was directly subjected to ion sieve adsorption to extract lithium without pH adjustment. Its lithium ion content was only reduced by 32.98 times, and the purity of the obtained sodium sulfate was only 98.28%, indicating that the filtrate after lithium precipitation was subjected to molecular sieve adsorption to extract lithium after pH adjustment, which can greatly improve the lithium ion adsorption efficiency. This may be because the filtrate is directly subjected to adsorbent lithium extraction, and the pH is higher and the alkaline environment is stronger, which will damage the adsorbent, resulting in a decrease in adsorption performance, thereby reducing the adsorption amount. It was also observed in the experiment that the adsorbent had a dissolution phenomenon. Moreover, the sodium sulfate in Example 1 is of higher purity, indicating that the use of H in the adsorbent can greatly improve the lithium ion adsorption efficiency. + Can achieve better impurity removal effect and Li + Get effective adsorption.
[0079] Comparative Example 2 (adjusting pH to 7 with acid)
[0080] 1.22g of 5% sodium hydroxide solution was added to 1L of lithium sulfate solution with a concentration of 220g / L until the pH value of the solution was 11.2, and then 0.86L of sodium carbonate solution with a concentration of 260g / L was added, and the reaction was carried out at a temperature of 85°C for 0.5h. After the reaction, a filtering operation was performed to obtain lithium carbonate and a filtrate, and the lithium carbonate was washed three times with deionized water to obtain 130.91g of lithium carbonate with a purity of 99.31%. 350.31g of 10wt% sulfuric acid was added to the filtrate obtained by the reaction to adjust the pH, and the pH value was adjusted to 7. The lithium ion concentration of the filtrate was measured to be 1.904g / L. The filtrate obtained by adjusting the pH was passed through a manganese dioxide ion sieve in the same manner as in Example 1 for adsorption and extraction of lithium. The sodium sulfate solution obtained by adsorption and extraction of lithium was tested, and its lithium content was reduced to 635mg / L, and its lithium ion content was only reduced by 3 times.
[0081] The sodium sulfate solution after adsorption was evaporated, crystallized, washed and dried to obtain 311.69g of sodium sulfate with a purity of 95.78%. Compared with Example 1, the total sulfuric acid dosage of Comparative Example 2 is 0.357mol, the total sulfuric acid dosage of Example 1 is 0.102mol, and the sulfuric acid dosage of Comparative Example 2 is greatly increased by 250%. After the molecular sieve is adsorbed, the lithium ion content in the solution still remains high, indicating that the lithium absorption effect is poor, which may be mainly due to the initial pH being neutral. As the H + The displacement causes the entire system to change in the acidic direction, reducing the adsorption capacity of the adsorbent; and the purity of sodium sulfate is low, and the impurity removal effect is also poor. The main reason for the low purity of the obtained sodium sulfate is that the residual lithium ions that have not been adsorbed in the solution enter the sodium sulfate.
[0082] Table 1
[0083]
[0084] Combined with Table 1, by comparing Examples 1 and 2 with Comparative Example 1, it can be seen that in Comparative Example 1, the lithium precipitation filtrate is directly subjected to lithium ion adsorbent without pH adjustment treatment, the alkalinity is too strong, and the lithium extraction effect is poor. This may be due to the excessive alkalinity, which causes damage to the adsorbent; and the purity of sodium sulfate in Comparative Example 1 is also low, indicating that the use of H in the adsorbent + CO3 2- The impurity removal effect is better.
[0085] By comparing Examples 1 and 2 with Comparative Example 2, it can be seen that when the pH is controlled in the range of 8-10, the lithium extraction effect is significantly improved, which may be due to the removal of H + After that, with CO3 2- Combined, so that the entire adsorption of Li + During the process, the adsorbent is under suitable alkaline conditions, so it has better adsorption performance; and the purity of sodium sulfate is also better, because not only Li + Effective adsorption and CO3 2- The H + and the amount of acid added in the lithium precipitation filtrate of the embodiment is also very small, such as the acid added in the comparative example to adjust the pH to 7-8, will consume a large amount of sulfuric acid.
[0086] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for recovering residual lithium in the lithium carbonate precipitation filtrate in the lithium sulfate precipitation process, characterized in that: The lithium sulfate precipitation lithium carbonate process comprises: subjecting lithium sulfate solution to lithium precipitation reaction with sodium hydroxide solution and sodium carbonate solution, filtering to obtain crude lithium carbonate and lithium precipitation filtrate; The recovery method comprises at least the following steps: S100, adding acid to the lithium precipitation filtrate to adjust the pH to 8-10, and then adding an adsorbent to adsorb and extract lithium to obtain a sodium sulfate solution and a lithium-containing adsorbent; S200, removing lithium from the lithium-containing adsorbent with acid to obtain a crude lithium chloride solution; S300, alkalizing and removing impurities from the crude lithium chloride solution, filtering, and obtaining a filtrate; The filtrate contains Li + , Cl - and impurity cations; S400, subjecting the filtrate to a first evaporation crystallization to obtain crude lithium chloride crystals, dissolving the crude lithium chloride crystals in an organic solvent, filtering, and obtaining a solid containing Li + and Cl - of recovery fluid; S500, subjecting the recovered liquid to a second evaporation crystallization to obtain high-purity lithium chloride.
2. The recycling method according to claim 1, characterized in that: The concentration of lithium ions in the lithium precipitation filtrate is 1.8 g / L to 2.0 g / L.
3. The recycling method according to claim 1, characterized in that: In step S100, acid is added to the sodium sulfate solution, and high-purity anhydrous sodium sulfate is obtained by evaporation and crystallization.
4. The recycling method according to claim 1 or 2, characterized in that: In step S100, the acid added to the lithium precipitation filtrate includes a sulfuric acid solution, and the mass concentration of the sulfuric acid solution is 1wt% to 10wt%.
5. The recycling method according to claim 1, characterized in that: In step S100, the adsorbent is a lithium ion adsorbent, which includes any one of manganese dioxide ion sieve, titanium oxide ion sieve, high-valent amorphous phosphate, hydrated SnO2, and amorphous Al(OH)3; Preferably, the adsorbent is a manganese dioxide ion sieve, and the lithium precipitation filtrate after pH adjustment flows through the manganese dioxide ion sieve at a flow rate of 3BV / h to 4BV / h for adsorption and lithium extraction. The manganese dioxide ion sieve is granular and has a bulk density of 70g / cm 3 Up to 75g / cm 3 ;or, Preferably, the adsorbent is titanium oxide ion sieve, and the lithium precipitation filtrate after pH adjustment flows through the titanium oxide ion sieve at a flow rate of 5BV / h to 7BV / h for adsorption and lithium extraction. The titanium oxide ion sieve is in powder form, 90% of which has a particle size between 1μm and 3μm, and an average particle size of 1.6μm to 1.8μm.
6. The recycling method according to claim 1, characterized in that: In step S200, the acid-eluting lithium removal includes: mixing the lithium-containing adsorbent and a hydrochloric acid solution to perform a lithium removal reaction, wherein the concentration range of the hydrochloric acid solution is 0.01 mol / L to 1 mol / L, and the adsorbent after lithium removal is returned to step S100 to continue to adsorb and extract lithium.
7. The recycling method according to claim 1, characterized in that: In step S300, the alkalization and impurity removal includes: adding alkali to the crude lithium chloride solution to adjust the pH to 7-8; Preferably, in step S300, the alkali used in the alkalization and impurity removal includes at least one of a sodium hydroxide solution, a lithium hydroxide solution, and a sodium carbonate solution; Further preferably, the alkali used in the alkalization and impurity removal comprises a sodium hydroxide solution with a mass content of 20wt% to 25wt%.
8. The recycling method according to claim 1, characterized in that: In step S400, the organic solvent is selected from anhydrous ethanol and / or anhydrous acetone.
9. The recycling method according to claim 1, characterized in that: In step S500, the organic solvent obtained by the second evaporation and crystallization of the recovered liquid is returned to step S400 to dissolve the crude lithium chloride crystals; Wherein, the temperature range of the second evaporation crystallization is 100°C to 280°C.
10. The recycling method according to claim 1, characterized in that: In the lithium sulfate precipitation lithium carbonate process, the concentration of the lithium sulfate solution is 200g / L to 260g / L, and the concentration of the sodium carbonate solution is 150g / L to 300g / L; Preferably, the molar ratio of sodium carbonate in the sodium carbonate solution to lithium sulfate in the lithium sulfate solution is 1.0 to 1.2; Further preferably, the conditions for the lithium precipitation reaction include: Lithium deposition temperature: 15℃~98℃; Reaction time: 0.2h~3h.
Citation Information
Patent Citations
Technology for extracting high-purity lithium chloride from lithium ore
CN106365180A
Method for recovering lithium in lithium carbonate lithium precipitation mother liquor
CN111533146A
Method for preparing battery-grade lithium phosphate from lithium-containing brine
CN117945373A
Method and system for extracting lithium from lithium-containing brine to prepare lithium carbonate
CN118221142A
Cited By
Lithium carbonate separation process for freezing, evaporating, thermally crystallizing and decarburizing liquid after lithium precipitation
CN120964850A
A method and process system for efficient lithium extraction and resource utilization from low- to medium-grade lithium-containing brines
CN121342055B