Resource utilization method of minerals with low aluminum-silicon ratio
Through the roasting activation, metathesis and caustic treatment of low-aluminum-silicon minerals, the problem of insufficient resource utilization is solved, the preparation of high-silicon-aluminum-silicon minerals and the production of calcium silicate are realized, which meets the production needs of alumina and realizes the realization of the production of alumina. Efficient recycling of resources.
Patent Information
- Application Number
- CN202410989819.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
China has a scarce bauxite resources, and the aluminum-silicon ratio of low-grade bauxite and high-aluminum-gangue gangue is not sufficient to meet the requirements of Bayer method for producing alumina, and these resources cannot be effectively utilized.
By calcining and activation of low aluminum-silicon ratio minerals with an aluminum-silicon ratio of 1 to 6, then metathesis reaction with alkali solution, reducing the silicon content and increasing the aluminum-silicon ratio, then precipitation reaction with CO2, and finally causticizing with lime. Generate high silicon-aluminum-specific minerals and calcium silicates that meet the requirements of Bayer method.
Resource utilization of low aluminum-silicon ratio minerals was achieved, high silicon-aluminum ratio minerals that meet the requirements of alumina production were prepared, and strong alkali solution was returned to metathesis reaction, realizing recycling, and improving the integration of aluminum-silicon ratio and resources. Utilization efficiency.
Smart Images

Figure CN118929713A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of mineral resource utilization, and in particular to a resource utilization method for low aluminum-silicon ratio minerals. Background Art
[0002] China is the largest producer and consumer of alumina, but its bauxite resources are not abundant and it needs to import a large amount of bauxite from abroad. However, there are a large number of low-grade bauxite and high-aluminum coal gangue stored in China, and the reserves are huge. However, the aluminum-silicon ratio of low-grade bauxite is only 1-6, and the aluminum-silicon ratio of high-aluminum coal gangue is only 1-4, which cannot meet the requirements of Bayer process for producing alumina (the aluminum-silicon ratio must be greater than 6). Summary of the invention
[0003] The purpose of the present invention is to provide a method for resource utilization of low aluminum-silicon ratio minerals, and the present invention realizes resource utilization of low aluminum-silicon ratio minerals.
[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0005] The present invention provides a method for resource utilization of low aluminum-silicon ratio minerals, comprising the following steps:
[0006] The low aluminum-silicon ratio mineral with an aluminum-silicon ratio of 1 to 6 is roasted and activated to obtain a roasted activated ore;
[0007] At room temperature and pressure, the roasted activated ore is mixed with an alkaline solution to undergo double decomposition reaction to obtain a crude silicate solution and a high aluminum-silicon ratio mineral with an aluminum-silicon ratio higher than 6;
[0008] The crude silicate solution is mixed with roasted activated ore, CO 2 Mixing and performing precipitation reaction to obtain a refined silicate solution;
[0009] The refined silicate solution is mixed with lime for causticization to obtain a strong alkaline solution and calcium silicate.
[0010] Preferably, the low aluminum-silicon ratio mineral includes one or more of low-grade bauxite, medium-grade bauxite and high-aluminum coal gangue.
[0011] Preferably, the particle size of the low aluminum-silicon ratio mineral is less than 1 mm.
[0012] Preferably, in terms of mass fraction, the low silicon-aluminum ratio mineral includes Al 2 O 3 33.86~37.57%、SiO 2 40.11~42.49%, CaO 0.07~0.14%, Fe 2 O 3 0.34~0.47%、Na 2O 0.22~0.47%、TiO 2 0.7~0.95% and the rest impurities
[0013] Preferably, the calcination activation temperature is 950-1100° C. and the time is 0.3-20 min.
[0014] Preferably, the liquid-to-solid ratio of the roasted activated ore to the alkaline solution is 2 to 8:1; and the concentration of the alkali in the alkaline solution is 90 to 150 g / L.
[0015] Preferably, the temperature of the double decomposition reaction is 80-110° C., and the time is 10-90 min.
[0016] Preferably, the mass ratio of the crude silicate solution to the roasted activated ore is 50 to 280:1.
[0017] Preferably, the molar ratio of the refined silicate solution to lime is 0.4-2:1; and the concentration of the refined silicate solution is 90-150 g / L.
[0018] Preferably, the causticizing temperature is 70-110° C. and the time is 10-60 min.
[0019] The present invention provides a method for resource utilization of low aluminum-silicon ratio minerals, comprising the following steps:
[0020] The low aluminum-silicon ratio mineral with an aluminum-silicon ratio of 1 to 6 is roasted and activated to obtain a roasted activated ore;
[0021] At room temperature and pressure, the roasted activated ore is mixed with an alkaline solution to undergo double decomposition reaction to obtain a crude silicate solution and a high aluminum-silicon ratio mineral with an aluminum-silicon ratio higher than 6;
[0022] The crude silicate solution is mixed with roasted activated ore, CO 2 Mixing and performing precipitation reaction to obtain a refined silicate solution;
[0023] The refined silicate solution is mixed with lime for causticization to obtain a strong alkaline solution and calcium silicate.
[0024] The silicon dioxide in the low aluminum-silicon ratio mineral is mostly in the form of kaolinite (soil), which has perfect and dense crystals and is not easy to react with strong alkaline solutions. The present invention uses the low aluminum-silicon ratio mineral for roasting and activation. During the roasting and activation process, the kaolinite undergoes a decomposition reaction, which reduces the density and improves its chemical reaction activity, and then reduces the silicon content through a double decomposition reaction; and the aluminum oxide in the roasted activated ore hardly reacts with sodium hydroxide at room temperature and pressure, thereby improving the aluminum-silicon ratio of the product, and preparing a high silicon-aluminum ratio mineral that meets the requirements of the Bayer process for producing aluminum oxide. In addition, the high silicon-aluminum ratio mineral can also be used as a mineral raw material for deep desiliconization, and further improves the aluminum-silicon ratio for use in aluminum oxide production; and calcium silicate is prepared using the low aluminum-silicon ratio mineral, realizing the resource utilization of the low aluminum-silicon ratio mineral. In addition, the prepared strong alkaline solution can be reused in the double decomposition reaction to achieve recycling. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The process flow chart of an embodiment of the present invention. DETAILED DESCRIPTION
[0026] The present invention provides a method for resource utilization of low aluminum-silicon ratio minerals, comprising the following steps:
[0027] The low aluminum-silicon ratio mineral with an aluminum-silicon ratio of 1 to 6 is roasted and activated to obtain a roasted activated ore;
[0028] At room temperature and pressure, the roasted activated ore is mixed with an alkaline solution to undergo double decomposition reaction to obtain a crude silicate solution and a high aluminum-silicon ratio mineral with an aluminum-silicon ratio higher than 6;
[0029] The crude silicate solution is mixed with roasted activated ore, CO 2 Mixing and performing precipitation reaction to obtain a refined silicate solution;
[0030] The refined silicate solution is mixed with lime for causticization to obtain a strong alkaline solution and calcium silicate.
[0031] The invention roasts and activates a low aluminum-silicon ratio mineral with an aluminum-silicon ratio of 1 to 6 to obtain a roasted activated ore.
[0032] In the present invention, the low aluminum-silicon ratio mineral preferably includes one or more of low-grade bauxite, medium-grade bauxite and high-aluminum coal gangue; the particle size of the low aluminum-silicon ratio mineral is less than 1 mm, and D50 is preferably 74 μm.
[0033] In the present invention, the low silicon-aluminum ratio mineral preferably includes Al 2 O 3 33.86~37.57%、SiO 2 40.11~42.49%, CaO 0.07~0.14%, Fe2 O 3 0.34~0.47%、Na 2 O0.22~0.47%、TiO 2 0.7~0.95% and the balance impurities.
[0034] In the present invention, the resource utilization method of the low aluminum-silicon ratio mineral preferably comprises: successively crushing and grinding the low aluminum-silicon ratio mineral raw material.
[0035] The present invention has no special limitation on the equipment used for crushing and grinding, and conventional crushing and grinding equipment can be used.
[0036] In the present invention, the temperature of the calcination activation is preferably 950-1100°C, more preferably 1050-1080°C; the calcination time is 0.3-20 min, more preferably 5-18 min, and further preferably 10-15 min. In the present invention, the calcination activation is preferably carried out in a fluidized furnace and / or a suspension calcination furnace. Calcination activation can cause a decomposition reaction of a low aluminum-silicon ratio mineral, reduce its density, and increase its chemical reactivity.
[0037] After obtaining the roasted activated ore, the present invention mixes the roasted activated ore with a strong alkali solution at room temperature and pressure to perform double decomposition reaction to obtain a crude silicate solution and a high aluminum-silicon ratio mineral with an aluminum-silicon ratio higher than 6.
[0038] In the present invention, the liquid-to-solid ratio of the roasted activated ore to the alkaline solution is preferably 2-8:1, more preferably 3-6:1, and the liquid-to-solid ratio refers to the mass ratio of the roasted activated ore to the alkaline solution; the concentration of the alkali in the alkaline solution is preferably 90-150 g / L, more preferably 120-130 g / L; the alkali preferably includes sodium hydroxide and / or potassium hydroxide.
[0039] In the present invention, the temperature of the metathesis reaction is preferably 80-110°C, more preferably 80-90°C; the time is preferably 10-90 min, more preferably 20-60 min, more preferably 25-35 min. In the present invention, the temperature of the metathesis reaction is preferably reached by steam heating; the steam is preferably saturated steam of 0.6 MPa.
[0040] In the double decomposition reaction, 40-70% of amorphous silica and part of Al in the mineral 2 O 3 ·2SiO 2 Reacts with alkaline solution to form silicate solution.
[0041] After the double decomposition reaction, the present invention preferably performs solid-liquid separation on the obtained double decomposition reaction product to obtain the crude silicate solution and a high aluminum-silicon ratio mineral with an aluminum-silicon ratio higher than 6.
[0042] In the present invention, the solid-liquid separation is preferably carried out in a cyclone, a centrifuge or a filter.
[0043] After obtaining the crude silicate solution, the present invention mixes the crude silicate solution with roasted activated ore, CO 2 The mixture is mixed to undergo a precipitation reaction to obtain a refined silicate solution.
[0044] In the present invention, the mass ratio of the crude silicate solution to the roasted activated ore is 50 to 280: 1, more preferably 100 to 240: 1, and further preferably 150 to 200: 1. The precipitation reaction removes some impurities.
[0045] After the precipitation reaction, the present invention preferably performs solid-liquid separation on the obtained precipitation reaction product to obtain the refined silicate solution.
[0046] In the present invention, the solid-liquid separation is preferably carried out in a sedimentation tank and / or a leaf filter.
[0047] After obtaining the refined silicate solution, the present invention mixes the refined silicate solution with lime milk for causticization to obtain a strong alkaline solution and calcium silicate.
[0048] In the present invention, the molar ratio of the refined silicate solution to lime is preferably 0.4-2:1, more preferably 0.5-1.5:1, and the concentration of the refined silicate solution is preferably 90-150 g / L, more preferably 100-120 g / L; the lime is preferably mixed with the refined silicate solution in the form of lime milk.
[0049] In the present invention, the causticizing temperature is preferably 70 to 110° C., more preferably 80 to 110° C., and further preferably 80 to 90° C.; the time is preferably 10 to 60 min, more preferably 30 to 40 min, and further preferably 25 to 35 min.
[0050] After causticizing, the present invention preferably separates the obtained causticizing product to obtain a low concentration strong alkaline solution and wet calcium silicate;
[0051] The low-concentration strong alkali solution is evaporated to obtain the alkali solution; the wet calcium silicate is dried to obtain the calcium silicate.
[0052] In the present invention, the separation is preferably carried out in a settling tank and / or a leaf filter.
[0053] In the present invention, the evaporation is preferably performed by heating with steam.
[0054] The flowchart of the embodiment of the present invention is as follows Figure 1As shown in the figure: a low aluminum-silicon ratio mineral is pretreated and then roasted and activated, the obtained roasted activated ore is mixed with sodium hydroxide and then desiliconized at normal pressure (i.e., double decomposition reaction) under steam heating; the desiliconized product is subjected to solid-liquid separation to obtain a high silicon-aluminum ratio compound and a crude sodium silicate solution; the crude sodium silicate solution is mixed with the roasted activated ore and carbon dioxide to remove impurities and filter to obtain a refined silicate solution; the refined silicate solution is mixed with lime milk and then causticized under steam heating, and then the causticized product is separated and filtered to obtain wet calcium silicate and a low-concentration alkali solution; the wet calcium silicate is dried to obtain calcium silicate; the low-concentration alkali solution is evaporated under steam heating, and the obtained alkali solution can be reused in the atmospheric pressure desiliconization.
[0055] The resource utilization method of low aluminum-silicon ratio minerals provided by the present invention is described in detail below in conjunction with the embodiments, but they should not be understood as limiting the scope of protection of the present invention.
[0056] Example 1
[0057] The low aluminum-silicon ratio mineral (in terms of mass fraction, the components are: Al 2 O 3 34.78%, SiO 2 40.11%, CaO 0.14%, Fe 2 O 3 0.41%, Na 2 O 0.31%, TiO 2 The ore is crushed to less than 10 mm by jaw crusher and cone crusher, and then ground by high pressure roller mill and ball mill to a particle size of less than 1 mm, with a D50 of 74 μm.
[0058] The low aluminum-silicon ratio mineral raw material is placed in a gas suspension roasting furnace and roasted and activated at 1050°C for 2 minutes to obtain a roasted activated ore.
[0059] 1 part of roasted activated ore was mixed with 4 parts of 125g / L sodium hydroxide solution to prepare slurry, which was heated to 97°C by 0.6MPa steam and desiliconized at normal pressure for 25 minutes. 40-70% of the silica and part of the Al in the slurry were 2 O 3 .SiO 2 Converted into sodium silicate solution.
[0060] The desiliconized ore pulp is separated by solid-liquid separation through cyclones and leaf filters. The solid is a high aluminum-silicon ratio compound that can enter the Bayer process to produce alumina, and the liquid phase is a crude sodium silicate solution.
[0061] Add CO to 100 parts of crude sodium silicate solution. 2 and 1 part roasted activated ore, CO 2It reacts with calcium ions in the crude sodium silicate solution to generate calcium carbonate precipitation, and the activated ore is roasted to serve as precipitation crystal seeds. The resulting product is then filtered through a sedimentation tank and a leaf filter to obtain a refined sodium silicate solution.
[0062] Add 1 part of lime milk to 1 part of refined sodium silicate solution (the molar ratio of sodium silicate to lime in the refined sodium silicate solution is 1:1), and heat to 90°C using 0.6MPa steam. After 15 minutes, the sodium silicate and calcium hydroxide react to generate calcium silicate and sodium hydroxide. The resulting product is then separated into solid and liquid through a sedimentation tank and a leaf filter. The obtained wet calcium silicate is applied to the papermaking industry after air flow drying or drum drying. The sodium hydroxide solution is indirectly heated and evaporated by 0.6MPa steam to increase the concentration of the alkali solution and return to normal pressure for desiliconization.
[0063] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.
Claims
1. A method for resource utilization of low aluminum-silicon ratio minerals, characterized in that: The following steps are involved: The low aluminum-silicon ratio mineral with an aluminum-silicon ratio of 1 to 6 is roasted and activated to obtain a roasted activated ore; At room temperature and pressure, the roasted activated ore is mixed with an alkaline solution to undergo double decomposition reaction to obtain a crude silicate solution and a high aluminum-silicon ratio mineral with an aluminum-silicon ratio higher than 6; The crude silicate solution is mixed with roasted activated ore and CO2 to perform precipitation reaction to obtain a refined silicate solution; The refined silicate solution is mixed with lime for causticization to obtain a strong alkaline solution and calcium silicate.
2. The resource utilization method according to claim 1, characterized in that: The low aluminum-silicon ratio mineral includes one or more of low-grade bauxite, medium-grade bauxite and high-aluminum coal gangue.
3. The resource utilization method according to claim 1 or 2, characterized in that: The particle size of the low aluminum-silicon ratio mineral is less than 1 mm.
4. The resource utilization method according to claim 1 or 2, characterized in that: Calculated by mass fraction, the low silicon-aluminum ratio mineral includes Al2O3 33.86-37.57%, SiO2 40.11-42.49%, CaO 0.07-0.14%, Fe2O3 0.34-0.47%, Na2O 0.22-0.47%, TiO2 0.7-0.95% and the remainder of impurities.
5. The resource utilization method according to claim 1, characterized in that: The calcination activation temperature is 950-1100° C. and the time is 0.3-20 minutes.
6. The resource utilization method according to claim 1, characterized in that: The liquid-to-solid ratio of the roasted activated ore to the alkaline solution is 2-8:1; and the concentration of the alkali in the alkaline solution is 90-150 g / L.
7. The resource utilization method according to claim 1 or 6, characterized in that: The temperature of the double decomposition reaction is 80-110° C., and the time is 10-90 minutes.
8. The resource utilization method according to claim 1, characterized in that: The mass ratio of the crude silicate solution to the roasted activated ore is 50 to 280:
1.
9. The resource utilization method according to claim 1, characterized in that: The molar ratio of the refined silicate solution to lime is 0.4-2:1; the concentration of the refined silicate solution is 90-150 g / L.
10. The resource utilization method according to claim 1 or 9, characterized in that: The causticizing temperature is 70-110° C. and the time is 10-60 minutes.
Citation Information
Cited By
Method for preparing artificial bauxite with high alumina-silica ratio by using minerals with low alumina-silica ratio
CN121491127A