Preparation method for preparing rare earth oxide by spray coprecipitation gel drying method
Rare earth oxide powders were prepared by spray co-precipitation gel drying, which solved the problem of poor sintering activity of rare earth oxide ceramics in the prior art, and achieved the preparation of rare earth oxide nano powder with good purity and dispersion, significantly improving the Laser output performance.
Patent Information
- Application Number
- CN202410885714.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-12
AI Technical Summary
During the sintering and preparation process, existing rare earth oxide Y2O3, Lu2O3 and Sc2O3 series transparent ceramics have problems such as wide particle size distribution, messy morphology, many impurities, and poor sintering activity, resulting in poor laser output or no laser output, which is difficult to meet the high level. Strict requirements for power lasers.
Rare earth oxide powder is prepared by spray co-precipitation gel drying method. By mixing metal ion solution with ammonium bicarbonate and ammonia water as precipitant at room temperature, near spherical nanopowder is prepared by ultrasonic wave and mechanical stirring, and then at a specific temperature. Under calcination, laser-grade transparent ceramics are formed with high purity and dispersibility.
The prepared rare earth oxide powder has uniform particle size, regular morphology, good dispersion, and high yield. It can be sintered at a lower temperature to prepare high-power laser-grade transparent ceramics, which significantly improves the laser output performance.
Smart Images

Figure CN118929730A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of optical functional transparent ceramics, and specifically relates to a method for preparing rare earth oxides by a spray coprecipitation gel drying method. Background Art
[0002] Transparent ceramics are widely used in lighting, optical windows, CT scintillators, solid laser gain media and other fields. Compared with lighting, optical windows and scintillators, laser gain media have the most stringent requirements on the quality of transparent ceramics: as few impurities and defects as possible, higher thermal conductivity, and lower thermal expansion coefficient to achieve laser output.
[0003] Rare earth doped yttrium aluminum garnet (chemical formula Y 3 Al 5 O 12 YAG (abbreviated as YAG) crystal is the most studied and widely used gain medium material for KW-level high-power lasers. However, due to its inherently low thermal conductivity and high thermal expansion coefficient, YAG is not the best matrix material for high-power lasers. In contrast, rare earth oxide Y 2 O 3 、Lu 2 O 3 Sc 2 O 3 The series of materials have higher thermal conductivity and are suitable for trivalent rare earth luminescent ions such as Yb 3+ 、Nd 3+ , Er 3+ 、Ho 3 + 、Tm 3+ etc. have better emission and absorption cross sections, which makes Y 2 O 3 、Lu 2 O 3 Sc 2 O 3 A series of transparent materials have become more promising gain media for high-power lasers.
[0004] Using rare earth oxide Y 2 O 3 、Lu 2 O 3 Sc 2 O 3 Both powder-prepared single crystals and transparent ceramics can be used as laser gain media. 2 O 3 、Lu 2 O 3 Sc 2 O 3The melting points are all above 2400℃, which makes the growth of single crystals of this series of oxides very difficult and the production cost is high. They are also used as laser gain media. 2 O 3 、Lu 2 O 3 Sc 2 O 3 The sintering temperature of the series of transparent ceramics is often below 1900℃, and the production cost is lower. Ceramics of the same material have better mechanical strength than single crystals and can achieve higher concentrations of ion doping. Therefore, Y 2 O 3 、Lu 2 O 3 Sc 2 O 3 A series of transparent ceramics are high-power laser gain medium materials with greater application potential.
[0005] Y 2 O 3 、Lu 2 O 3 Sc 2 O 3 There have been many reports on the research of a series of transparent ceramics. Currently, commercial powders or self-synthesized powders can be sintered at 1600-1900℃ to prepare this series of transparent ceramics with observation window-level optical quality. However, the existing commercial powders and self-synthesized powders have the disadvantages of wide particle size distribution, messy powder morphology, more impurities, serious agglomeration, and poor sintering activity. 2 O 3 、Lu 2 O 3 Sc 2 O 3 This series of transparent ceramics contain micropores, serious coarsening of ceramic grains, broad grain boundaries, and a large number of color centers. When used as gain media, the laser output is poor or even no laser output.
[0006] High-activity nanopowders with high purity, good dispersibility, uniform morphology and particle size, and no obvious agglomeration are the key to preparing high-power laser output gain media. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing rare earth oxides by a spray coprecipitation gel drying method. The series of powders prepared according to the present invention have a nearly spherical regular morphology, uniform particle size, good dispersibility, high activity, and a yield of ≥99%. The series of laser-grade optical quality transparent ceramics are prepared by sintering at 1400-1600°C.
[0008] To achieve the above purpose, the present invention prepares Y 2 O 3 、Lu 2O 3 Sc 2 O 3 The technical solutions of the series of nano powder methods include:
[0009] 4N purity Y 2 O 3 、Lu 2 O 3 Sc 2 O 3 The coarse powder is dissolved in an inorganic acid solution and diluted with ultrapure water to prepare a 0.1 mol / L-0.5 mol / L concentration corresponding metal ion solution;
[0010] A dispersant is added to each of the above metal ion solutions and stirred for 1-48 hours; a mixed solution of 0.5-2.5 mol / L ammonium bicarbonate and 0.5 mol / L-4.0 mol / L ammonia water is prepared with ultrapure water as a precipitant;
[0011] A spray device consisting of a peristaltic pump, an infusion silicone tube, 5N high-purity nitrogen, a plastic air pipe, and an ultrasonic generator full-plastic atomizing nozzle is used to spray the precipitant solution in the form of ultrafine droplets into a container containing 0.01-5% dispersant metal ion solution within 1-5 hours, and a mechanical stirrer is used with a tetrafluoroethylene stirring paddle for continuous stirring and multiple ultrasonic treatments to prepare a single precursor or mixed precursor slurry of yttrium, lutetium, and scandium, and the pH value of the slurry at the spray end point is 7.0-8.8;
[0012] After 4-30h stirring and ultrasonic aging, the precursor slurry is filtered and washed with ultrapure water and ethanol three times respectively to obtain a precursor precipitate;
[0013] The precursor precipitate is added to ethanol to obtain an ethanol-dispersed precursor slurry with a solid content of 10-50%, and various 0.001-5% gel dispersants are added, and the mixture is continuously stirred and ultrasonically aged for 5-24 hours, and then discharged through a discharge port;
[0014] The matured precursor ethanol slurry is heated and dried at 70-120°C to form a gel within 10-120 minutes after the start of heating. The slurry is dried for 24-50 hours to obtain an ultra-dispersed precursor precipitate dry material, which is sieved through 80-200 mesh and calcined in an air furnace at 1000-1300°C for 2-10 hours to form Y 2 O 3 、Lu 2 O 3 Sc 2 O 3 Series of nano powders.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] The raw material powder used in the present invention only needs to be of high purity, and has no requirements on the morphology of the particles. The coprecipitation preparation device is simple and can be prepared continuously, which is environmentally friendly. The obtained powder yield is ≥ 99%, and it is easy to scale up production. A single rare earth element or a mixed rare earth element oxide powder in any proportion can be prepared at will. The Y synthesized by the present invention 2 O 3 、Lu 2 O 3 Sc 2 O 3 The series of nanopowders can be directly used to prepare flawless high-power laser-grade transparent ceramics after simple treatment, which is suitable for the industrial production of ultra-high-quality rare earth oxide powders. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 A diagram of the coprecipitation preparation apparatus;
[0018] Figure 2 This is a physical picture of the gel sample of the precursor ethanol slurry heated at 100°C for 1h in Example 1;
[0019] Figure 3 Y obtained by calcining at 1300°C in Example 1 2 O 3 Powder XRD pattern;
[0020] Figure 4 Y prepared at 1300°C in Example 1 2 O 3 SEM morphology of powder;
[0021] Figure 5 For the Lu prepared at 1250°C in Example 2 2 O 3 SEM morphology of powder;
[0022] Figure 6 Sc prepared at 1150°C in Example 3 2 O 3 SEM morphology of powder;
[0023] Figure 7 For the LuScO prepared at 1100°C in Example 4 3 SEM morphology of powder;
[0024] Figure 8 Y obtained by using Example 1 and Example 2 2 O 3 、Lu 2 O 3 Powder firing corresponding Y 2 O 3 、Lu 2 O 3 Transparent ceramic figure.
[0025] In the figure: 1) 5N high-purity nitrogen, 2) precipitant and container, 3) peristaltic pump, 4) silicone tube, 5) plastic air tube, 7) metal ion solution and container, 8) all-plastic atomizing nozzle, 9) ultrasonic generator, 10) mechanical stirrer, 11) polytetrafluoroethylene stirring paddle, 12) discharge port. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Example 1: Y 2 O 3 Nanopowder synthesis
[0028] The yttrium oxide powder raw material is dissolved in an excess of 4% hydrochloric acid aqueous solution, filtered and diluted with water to form a 0.1 mol / L yttrium chloride solution, hydroxyethyl cellulose dispersant is added, and a mixed aqueous solution of 2 mol / L ammonium bicarbonate and 2.5 mol / L ammonia water is prepared and filtered as a precipitant, and the precipitant solution is added to the yttrium chloride solution in the form of a spray by a spray coprecipitation method, and the spray and subsequent stirring and aging process are supplemented by multiple ultrasonic dispersions to obtain a Y precursor slurry.
[0029] The precursor slurry was filtered, washed with ultrapure water for 4 times, and washed with ethanol for 4 times, and then redispersed in ethanol to prepare a slurry. Subsequently, cellulose, PEG600, and dextrin gel dispersant were added, and the slurry was matured by continuous stirring and multiple ultrasonic treatments.
[0030] The matured precursor ethanol slurry was heated at 100°C for 1 hour to complete gelation. Figure 2 Continue to heat at 80°C for 40 hours to dry, and sieve the precursor dry material with 200 mesh.
[0031] The precursor powder was calcined at 1300°C for 6 hours to obtain nano yttrium oxide powder. The XRD diffraction pattern of the yttrium oxide powder obtained in Example 1 is shown in the figure, and its SEM morphology is shown in the figure. It can be seen from the figure that Y 2 O 3 The powder particles are nearly spherical in shape, and the average particle size is around 200 nm.
[0032] Example 2: Lu 2 O 3 Nanopowder synthesis
[0033] The lutetium oxide powder raw material is dissolved in an excess of 2% nitric acid aqueous solution, filtered and diluted with water to form a 0.3 mol / L lutetium nitrate solution, hydroxypropyl methylcellulose dispersant is added, and a mixed aqueous solution of 2.5 mol / L ammonium bicarbonate and 2 mol / L ammonia water is prepared and filtered as a precipitant, and the precipitant solution is added to the lutetium nitrate solution in the form of a spray by a spray co-precipitation method, and the spray and subsequent stirring and aging process are supplemented by multiple ultrasonic dispersions to obtain a Lu precursor slurry.
[0034] The precursor slurry was filtered, washed with ultrapure water for 4 times, and washed with ethanol for 4 times, and then redispersed in ethanol to prepare a slurry. Subsequently, cellulose, PEG600, and dextrin gel dispersant were added, and the slurry was matured by continuous stirring and multiple ultrasonic treatments.
[0035] The matured precursor ethanol slurry was first heated at 110° C. for 40 min to complete gelation, and then heated at 90° C. for 40 h to dry, and the precursor dry material was sieved through a 180-mesh screen.
[0036] The precursor powder was calcined at 1250°C for 10 h to obtain nano-lutetium oxide powder. The SEM morphology of the lutetium oxide powder obtained in Example 2 is shown in the figure. 2 O 3 The powder particles are nearly spherical in shape and the average particle size is around 180nm.
[0037] Example 3: Sc 2 O 3 Nanopowder synthesis
[0038] The scandium oxide powder raw material is dissolved in an excess of 1% nitric acid aqueous solution, filtered and diluted with water to form a 0.4 mol / L scandium nitrate solution, methyl cellulose dispersant is added, and a mixed aqueous solution of 2.5 mol / L ammonium bicarbonate and 1.5 mol / L ammonia water is prepared and filtered as a precipitant. The precipitant solution is added to the scandium nitrate solution in the form of a spray by a spray co-precipitation method, and the spraying and subsequent stirring and aging process are supplemented by multiple ultrasonic dispersions to obtain a precursor slurry of Sc.
[0039] The precursor slurry was filtered, washed with ultrapure water for 4 times, and washed with ethanol for 4 times, and then redispersed in ethanol to prepare a slurry. Subsequently, cellulose, PEG600, and dextrin gel dispersant were added, and the slurry was matured by continuous stirring and multiple ultrasonic treatments.
[0040] The matured precursor ethanol slurry was first heated at 90°C for 60 minutes to complete gelation, and then heated at 90°C for 40 hours for drying, and then sieved with 200 mesh.
[0041] The precursor powder was calcined at 1150°C for 10 hours to obtain nano scandium oxide powder. 2 O 3The powder particles are nearly spherical in shape and the average particle size is around 120 nm.
[0042] Example 4: LuScO 3 Nanopowder synthesis
[0043] The lutetium oxide and scandium oxide powder raw materials are dissolved in an excess 3% nitric acid aqueous solution at a molar ratio of 1:1, filtered and diluted with water to form a 0.4 mol / L lutetium scandium nitrate solution, hydroxypropyl cellulose dispersant is added, and a mixed aqueous solution of 2 mol / L ammonium bicarbonate and 2 mol / L ammonia water is prepared and filtered as a precipitant, and the precipitant solution is added to the lutetium scandium nitrate solution in the form of a spray by a spray co-precipitation method, and the spray and subsequent stirring and aging process are supplemented by multiple ultrasonic dispersions to obtain a precursor slurry of LuSc.
[0044] The precursor slurry was filtered, washed with ultrapure water for 4 times, and washed with ethanol for 4 times, and then redispersed in ethanol to prepare a slurry. Subsequently, cellulose, PEG600, and dextrin gel dispersant were added, and the slurry was matured by continuous stirring and multiple ultrasonic treatments.
[0045] The matured precursor ethanol slurry was first heated at 90°C for 60 minutes to complete gelation, and then heated at 90°C for 40 hours for drying, and then sieved with 200 mesh.
[0046] The precursor powder was calcined at 1100°C for 8 hours to obtain nano-lutetium-scandium oxide powder. The SEM morphology of the lutetium-scandium oxide powder obtained in Example 2 is shown in the figure. 3 The powder particles are nearly spherical in shape and the average particle size is around 80nm.
[0047] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0048] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing rare earth oxides by spray coprecipitation gel drying method, characterized in that: The preparation method comprises the following steps: S1: The raw material coarse powders of Y2O3, Lu2O3 and Sc2O3 are heated and dissolved in nitric acid or hydrochloric acid aqueous solution respectively, filtered as metal ion mother liquor, and then a non-ionic dispersant is added and stirred continuously; S2: preparing a mixed aqueous solution of ammonium bicarbonate and ammonia water, filtering it and using it as a precipitant; S3: When performing the spray coprecipitation reaction, the precipitant solution is suspended and sprayed into the continuously stirred metal ion mother solution in the form of ultrafine droplets and ultrasonically assisted dispersion is performed multiple times. The spraying is stopped when the pH value of the precursor slurry reaches 7.0-8.8, and stirring is continued for 4-30 hours to complete aging. This process is assisted by multiple ultrasonic dispersions; S4: The aged precursor slurry is filtered, washed with ultrapure water and ethanol for 2-4 times respectively to obtain a precursor precipitate; S5: Re-dispersing the precursor precipitate with ethanol to form a precursor ethanol slurry, adding a gel dispersant to the precursor ethanol slurry, and completing aging through continuous stirring and multiple ultrasonic treatments for 5-30 hours; S6: Heat and dry the matured precursor ethanol slurry in an oven, and form a gel within 10-40 minutes after the start of heating. Continue drying for 24-50 hours to obtain an ultra-dispersed precursor dry material, sieve it through 80-200 mesh, and calcine it in an air furnace for 2-10 hours to obtain Y2O3, Lu2O3, and Sc2O3 series nanopowders with an average particle size of 50-500nm.
2. The method for preparing rare earth oxides by spray coprecipitation gel drying method according to claim 1, characterized in that: In the step S1, the purity of the coarse powders of Y2O3, Lu2O3 and Sc2O3 raw materials is 4N, the inorganic acid used is one of nitric acid and hydrochloric acid, the purity of nitric acid and hydrochloric acid is GR or higher, the excess acid used for dissolution is 0-8%, and the heating temperature of the dissolution process is preferably 50-80°C.
3. The method for preparing rare earth oxides by spray coprecipitation gel drying method according to claim 2, characterized in that: The dispersant in step S1 and step S5 is one or more of methyl cellulose, hydroxymethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, dextrin, and PEG600.
4. The method for preparing rare earth oxides by spray coprecipitation gel drying method according to claim 1, characterized in that: The pore size of the filter membrane used to filter the metal ion nitrate or chloride solution in step S1 is preferably 0.05-1 micron, and the pore size of the filter membrane used to filter the precipitant solution in step S2 is preferably 0.05-1 micron.
5. The method for preparing rare earth oxides by spray coprecipitation gel drying method according to claim 4, characterized in that: The concentration of each metal ion solution prepared in step S1 is preferably 0.1-0.5 mol / L, the concentration of ammonium bicarbonate prepared as the precipitant in step S2 is preferably 0.5-2.5 mol / L, and the concentration of ammonia water is preferably 0.5-4 mol / L.
6. The method for preparing rare earth oxides by spray coprecipitation gel drying method according to claim 1, characterized in that: In step S3, the precipitant spray covers 30-90% of the surface area of the metal ion solution, the average particle size of the spray droplets is less than 100 microns, and the total spray time used for the pH value of the precursor slurry to reach 7.0-8.8 is preferably 1-5 hours, and the spray time does not vary with the production scale.
7. The method for preparing rare earth oxides by spray coprecipitation gel drying method according to claim 1, characterized in that: The amount of dispersant added in step S1 is preferably 0.01-5%, and the amount of dispersant added in step S5 is preferably 0.001-5%.
8. The method for preparing rare earth oxides by spray coprecipitation gel drying method according to claim 1, characterized in that: The solid content of the precursor ethanol slurry in step S5 is preferably 10-50%.
9. The method for preparing rare earth oxides by spray coprecipitation gel drying method according to claim 1, characterized in that: In step S6, the oven temperature is preferably 70-120° C., and the precursor calcination temperature in an air furnace is preferably 900-1300° C.
10. The method for preparing rare earth oxides by spray coprecipitation gel drying method according to claim 1, characterized in that: In the ultrasound-assisted dispersion process of step S3 and step S5, a single ultrasound duration is 30-300 seconds, and an ultrasound interval is 20-60 minutes.