Method for removing fluorine and COD (Chemical Oxygen Demand) in vulcanized liquid of wastewater in copper smelting process

By using potassium permanganate and coagulant aids, the problems of fluoride and COD treatment in copper smelting wastewater were solved, achieving efficient fluoride removal and COD degradation, reducing wastewater treatment costs, and simplifying the process.

CN118929943AActive Publication Date: 2024-11-12JIANGXI COPPER GRP (GUIXI) SMELTING NEW TECH CO LTD

Patent Information

Application Number
CN202410949855.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-12
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

Existing technologies for treating wastewater from copper smelting processes suffer from problems such as prolonged fluoride removal processes, generation of large amounts of fluoride-containing waste residue, and high COD treatment costs. A method is needed to improve fluoride removal efficiency and depth while reducing wastewater treatment costs.

Method used

Potassium permanganate was reacted with the sulfidation liquid of copper smelting process wastewater, and a coagulant was added to form a flocculant. The precipitate and purified liquid were removed by filtration. Potassium permanganate promoted the transformation of sodium fluorosilicate into a precipitate form and degraded COD.

Benefits of technology

It improves the efficiency and depth of fluoride removal, degrades COD, reduces calcium ion deposition and scaling, lowers wastewater treatment costs, and is simple to operate and easy to industrialize.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929943A_ABST
    Figure CN118929943A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of wastewater treatment, and particularly discloses a method for removing fluorine and COD (Chemical Oxygen Demand) in a copper smelting process wastewater after-vulcanization liquid, which comprises the following steps: firstly, calculating the dosage of potassium permanganate required by reaction with sodium fluosilicate in the copper smelting process wastewater after-vulcanization liquid, then adding the potassium permanganate into the copper smelting process wastewater after-vulcanization liquid, heating and stirring, the method comprises the following steps: mixing sodium fluosilicate with water to obtain a mixed solution, adding a coagulant aid into the mixed solution, carrying out a mixing and stirring reaction to obtain a flocculated solution, filtering the flocculated solution to obtain a nickel-containing precipitate and a purified solution, introducing potassium permanganate to promote transformation of sodium fluosilicate, and separating a fluorine-containing compound from a system in a precipitate form. The newly generated sodium permanganate can effectively degrade COD (Chemical Oxygen Demand) in the wastewater, so that the defluorination efficiency and depth are improved, the degradation of COD is also helped to a certain extent, and a certain wastewater treatment cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wastewater treatment, and in particular relates to a method for removing fluorine and COD from sulfided wastewater from a copper smelting process, which is applicable to non-ferrous metallurgical wastewater treatment technology. Background Art

[0002] The main source of fluoride-containing wastewater is the flue gas purification process. In the process of washing smelting flue gas in the purification process, water glass is generally used to transfer the fluorine in the flue gas from the gas phase to the liquid phase, resulting in wastewater with a high fluorine content (fluorine content is 1000-6000 mg / L). Wastewater is generally first pre-treated by sulfidation, and most heavy metal pollutants are removed by adding sodium hydrosulfide solution, while fluorine-containing compounds and fluoride ions cannot be completely removed at this stage, and then neutralized by adding lime milk solution. Since sodium fluorosilicate reacts with alkali, the fluorine fixed in the water glass is redissolved into the wastewater, and then the precipitation method is used to make fluoride ions and calcium ions generate calcium fluoride precipitate to remove most of the fluorine.

[0003] Although the above process can remove most of the fluorine in the wastewater, it prolongs the fluorine removal process, produces a large amount of fluorine-containing waste slag, and increases the difficulty of subsequent treatment of the waste slag. The existing process does not treat the COD in the wastewater, and COD needs to be treated separately, resulting in an increase in the cost of wastewater treatment. Therefore, we need to propose a method for removing fluorine and COD from the liquid after sulfidation of copper smelting process wastewater to solve the above problems, so that it can greatly reduce the addition of calcium ions, improve the efficiency and depth of fluorine removal, and also help to degrade COD to a certain extent, thereby reducing certain wastewater treatment costs. Summary of the invention

[0004] The purpose of the present invention is to provide a method for removing fluorine and COD from the sulfided liquid of copper smelting process wastewater, which can greatly reduce the addition of calcium ions, improve the efficiency and depth of fluorine removal, and also help to degrade COD to a certain extent, thereby reducing a certain wastewater treatment cost, so as to solve the problems raised in the above-mentioned background technology.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for removing fluorine and COD from sulfided copper smelting wastewater, comprising the following steps:

[0007] S1. Calculate the amount of potassium permanganate required to react with sodium fluorosilicate based on the total content of sodium fluorosilicate in the sulfided copper smelting process wastewater;

[0008] S2, adding potassium permanganate to the sulfided liquid of copper smelting process wastewater, heating and stirring, and fully mixing and reacting to obtain a mixed solution;

[0009] S3, add a coagulant to the mixed solution and stir thoroughly, stir evenly and let stand for 10-30 minutes to obtain a flocculated solution;

[0010] S4. Filter the flocculated liquid to obtain a precipitate containing nickel and a purified liquid.

[0011] Preferably, in step S1, the amount of potassium permanganate is calculated as follows:

[0012] A1. Determine the molar mass of sodium fluorosilicate (M_Na2SiF6);

[0013] A2. Calculate the amount of sodium fluorosilicate (n_Na2SiF6) by dividing the total content of sodium fluorosilicate by the molar mass, with the total content in grams.

[0014] A3. According to the chemical reaction equation, determine the molar ratio of potassium permanganate to sodium fluorosilicate (a);

[0015] A4. Calculate the amount of potassium permanganate required (n_KMnO4): n_KMnO4 = a*n_Na2SiF6;

[0016] A5. Determine the molar mass of potassium permanganate (M_KMnO4);

[0017] A6. Calculate the mass of potassium permanganate required (m_KMnO4): m_KMnO4=n_KMnO4*M_KMnO4.

[0018] Preferably, in step S2, the molar ratio of the amount of potassium permanganate added to the amount of sodium fluorosilicate in the sulfided liquid of the copper smelting process wastewater is 1.5-5:1.

[0019] Preferably, the reaction conditions for adding potassium permanganate to the sulfided copper smelting process wastewater are: reaction temperature is 70-100° C., and reaction time is 3-12 h.

[0020] Preferably, when the potassium permanganate reacts with the sulfided liquid of copper smelting process wastewater, the potassium permanganate reacts with organic matter in the wastewater to oxidize the organic matter into carbon dioxide and water.

[0021] Preferably, in step S3, the coagulant aid is set to polyacrylamide with a molecular weight of 8 million to 18 million.

[0022] Preferably, the mixed solution is added with a coagulant to carry out flocculation reaction, the amount of the coagulant added is 1-5 mL / (L·sulfurized liquid), the mass fraction of the coagulant is 0.1%-0.5%, and the conditions of the flocculation reaction are: reaction time is 1-5 min, and reaction temperature is 20-25°C.

[0023] Preferably, when the coagulant is added, the coagulant is added to the mixed liquid by pumping, and then the mixed liquid is quickly stirred at a stirring rate of 400-800r / min using a stirring device to make the coagulant evenly dispersed in the liquid. After stirring for 1-5 minutes, the stirring speed is reduced to 200-300r / min, and the mixed liquid is slowly stirred for 1-5 minutes. After stirring, the mixed liquid is allowed to stand for 10-30 minutes to allow the flocs to have enough time to settle to the bottom of the container.

[0024] Preferably, in step S4, the precipitate needs to be subjected to nickel recovery, and the specific operation is as follows:

[0025] B1. Mix the nickel-containing precipitate with hydrochloric acid or nitric acid solution to dissolve the nickel and obtain a leaching solution; this is usually carried out under heating and stirring conditions to improve the leaching efficiency.

[0026] B2, filtering the leaching solution through a filtering device to obtain an insoluble residue and a clear liquid;

[0027] B3, precipitating sodium hydroxide or potassium hydroxide in the clear solution to precipitate nickel as nickel hydroxide to obtain a precipitated nickel compound;

[0028] B4. Calcine the precipitated nickel compound at high temperature to convert it into nickel oxide or metallic nickel.

[0029] Preferably, the purified liquid needs to be purified, and the specific purification steps are as follows:

[0030] C1. Use activated carbon filtering equipment to filter and remove organic matter, heavy metal ions or pigments in the solution to obtain a filtrate;

[0031] C2. Perform reverse osmosis operation on the filtrate using a reverse osmosis device to remove dissolved solids and obtain reverse osmosis liquid;

[0032] C3, sterilizing the reverse osmosis liquid through ultraviolet disinfection equipment to obtain treated liquid;

[0033] C4: If the treated liquid meets the emission standards, it will be returned to the process for recycling. If the treated liquid does not meet the emission standards, it will be returned to C1.

[0034] The method for removing fluorine and COD from the sulfided copper smelting process wastewater proposed in the present invention has the following advantages compared with the prior art:

[0035] 1. The present invention calculates the amount of potassium permanganate required for reacting with sodium fluorosilicate in the sulfided liquid of copper smelting process wastewater, then adds potassium permanganate to the sulfided liquid of copper smelting process wastewater for heating and stirring to obtain a mixed solution, then adds a coagulant to the mixed solution for mixed and stirred reaction to obtain a flocculated liquid, and finally filters the flocculated liquid to obtain a precipitate containing nickel and a purified liquid. The introduction of potassium permanganate promotes the transformation of sodium fluorosilicate, and fluorine-containing compounds are separated from the system in the form of precipitation. The newly generated sodium permanganate can effectively degrade COD in the wastewater, improves the defluorination efficiency and depth, and also helps to degrade COD to a certain extent, thereby reducing a certain wastewater treatment cost.

[0036] 2. The present invention can reduce calcium ion deposition and scaling in the defluorination process, and the present invention has a simple operation method, a simple and reliable process, is easy to industrialize, and has important economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a flowchart of the present invention;

[0038] Figure 2 A flowchart of nickel recovery from a precipitate of the present invention;

[0039] Figure 3 The figure is a flowchart of the purification process of the purified liquid of the present invention. DETAILED DESCRIPTION

[0040] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0041] Example 1

[0042] The present invention provides Figure 1-3 A method for removing fluorine and COD from sulfided copper smelting wastewater is shown, comprising the following steps:

[0043] S1. Calculate the amount of potassium permanganate required to react with sodium fluorosilicate based on the total content of sodium fluorosilicate in the sulfided copper smelting process wastewater;

[0044] The calculation method of the potassium permanganate dosage is as follows:

[0045] A1. Determine the molar mass of sodium fluorosilicate (M_Na2SiF6);

[0046] A2. Calculate the amount of sodium fluorosilicate (n_Na2SiF6) by dividing the total content of sodium fluorosilicate by the molar mass, with the total content in grams.

[0047] A3. According to the chemical reaction equation, determine the molar ratio of potassium permanganate to sodium fluorosilicate (a);

[0048] A4. Calculate the amount of potassium permanganate required (n_KMnO4): n_KMnO4 = a*n_Na2SiF6;

[0049] A5. Determine the molar mass of potassium permanganate (M_KMnO4);

[0050] A6. Calculate the mass of potassium permanganate required (m_KMnO4): m_KMnO4=n_KMnO4*M_KMnO4.

[0051] S2, adding potassium permanganate to the sulfided liquid of copper smelting process wastewater, heating and stirring, and fully mixing and reacting to obtain a mixed solution;

[0052] The molar ratio of the amount of potassium permanganate added to the sodium fluorosilicate content in the copper smelting process wastewater sulfide liquid is 1.5-5:1, and the reaction conditions for adding potassium permanganate to the copper smelting process wastewater sulfide liquid for reaction are: reaction temperature is 70-100°C, and reaction time is 3-12h.

[0053] When the potassium permanganate reacts with the sulfided liquid of the copper smelting process wastewater, the potassium permanganate reacts with the organic matter in the wastewater to oxidize the organic matter into carbon dioxide and water, thereby reducing the content of organic pollutants in the wastewater and achieving COD degradation.

[0054] S3, add a coagulant to the mixed solution and stir thoroughly, stir evenly and let stand for 10-30 minutes to obtain a flocculated solution;

[0055] The coagulant aid is set to polyacrylamide with a molecular weight of 8 million to 18 million;

[0056] The mixed solution is added with a coagulant to carry out flocculation reaction. The amount of the coagulant added is 1-5 mL / (L·sulfurized liquid), the mass fraction of the coagulant is 0.1%-0.5%, and the conditions of the flocculation reaction are: reaction time is 1-5 min, and reaction temperature is 20-25° C.

[0057] When the coagulant is added, the coagulant is added to the mixed liquid by pumping, and then the mixed liquid is quickly stirred at a stirring rate of 400-800r / min using a stirring device to uniformly disperse the coagulant in the liquid. After stirring for 1-5 minutes, the stirring speed is reduced to 200-300r / min, and the mixed liquid is slowly stirred for 1-5 minutes. After the stirring is completed, the mixed liquid is allowed to stand for 10-30 minutes to allow the flocs to have enough time to settle to the bottom of the container.

[0058] S4. Filter the flocculated liquid to obtain a precipitate containing nickel and a purified liquid.

[0059] The precipitate needs to be recovered for nickel, and the specific operation is as follows:

[0060] B1. Mix the nickel-containing precipitate with hydrochloric acid or nitric acid solution to dissolve the nickel and obtain a leaching solution; this is usually carried out under heating and stirring conditions to improve the leaching efficiency.

[0061] B2, filtering the leaching solution through a filtering device to obtain an insoluble residue and a clear liquid;

[0062] B3, precipitating sodium hydroxide or potassium hydroxide in the clear solution to precipitate nickel as nickel hydroxide to obtain a precipitated nickel compound;

[0063] B4. Calcine the precipitated nickel compound at high temperature to convert it into nickel oxide or metallic nickel.

[0064] The purified liquid needs to be purified, and the specific purification steps are as follows:

[0065] C1. Use activated carbon filtering equipment to filter and remove organic matter, heavy metal ions or pigments in the solution to obtain a filtrate;

[0066] C2. Perform reverse osmosis operation on the filtrate using a reverse osmosis device to remove dissolved solids and obtain reverse osmosis liquid;

[0067] C3, sterilizing the reverse osmosis liquid through ultraviolet disinfection equipment to obtain treated liquid;

[0068] C4: If the treated liquid meets the emission standards, it will be returned to the process for recycling. If the treated liquid does not meet the emission standards, it will be returned to C1.

[0069] Example 2

[0070] According to the method provided in Example 1, the fluorine and COD recovery operation was actually performed on the sulfided liquid of the copper smelting process wastewater for the first time to confirm the recovery of fluorine and COD. The specific operation steps are as follows:

[0071] 1. Detect the fluorine (F) component and COD value in the sulfided copper smelting process wastewater. The values ​​are shown in the following table:

[0072] Element Type F(mg / L) COD(mg / L) content 1200 1126

[0073] 2. Calculate the dosage of potassium permanganate as follows:

[0074] 21. The molar ratio of the amount of potassium permanganate added to the sodium fluorosilicate content in the copper smelting process wastewater after sulfidation is 1.5:1. Knowing the ratio of the molar mass of F in sodium fluorosilicate to the overall molar mass of sodium fluorosilicate, it can be known that the molar mass of sodium fluorosilicate (M_Na2SiF6) is 188.07 g / mol. The details are as follows:

[0075] M(Na2SiF6)=2*M(Na)+M(Si)+6*M(F)

[0076] =2*22.99+28.09+6*19.00

[0077] =45.98+28.09+114.00

[0078] =188.07 g / mol

[0079] Since the chemical formula of sodium fluorosilicate is Na2SiF6, we can see that there are 6 F atoms in each molecule. Therefore, the total molar mass ratio of F in sodium fluorosilicate is:

[0080] Ratio = 6*M(F) / M_Na2SiF6

[0081] =6*19.00 / 188.07

[0082] =114.00 / 188.07

[0083] =0.606 (approximately equal to)

[0084] 22. Calculate the total content of sodium fluorosilicate:

[0085] m_Na2SiF6=F content / F ratio

[0086] =1200mg / L / 0.606

[0087] ≈1980.49mg / L

[0088] 23. Calculate the amount of potassium permanganate required to react with it (n_KMnO4):

[0089] n_KMnO4=a*n_Na2SiF6

[0090] =1.5*(m_Na2SiF6 / M_Na2SiF6)

[0091] =1.5*(1980.49mg / L / 188.07g / mol)

[0092] ≈1.5*(1.98049g / L / 188.07g / mol)

[0093] ≈1.5*0.01053mol / L

[0094] ≈0.015795mol / L

[0095] 24. Calculate the mass of potassium permanganate required (m_KMnO4):

[0096] m_KMnO4=n_KMnO4*M_KMnO4

[0097] =0.015795mol / L*158.04g / mol

[0098] ≈2.513 g / L;

[0099] 3. Add potassium permanganate at a ratio of 2.513 g / L to the sulfided liquid of copper smelting process wastewater, heat and stir, fully mix and react to obtain a mixed solution, the reaction temperature is 70°C, the reaction time is 12 hours, and the fluorine (F) component and COD value in the reaction solution are detected. The values ​​are shown in the following table:

[0100] Element Type F(mg / L) COD(mg / L) content 1161.6 200

[0101] From this table, we can know that after potassium permanganate reaction, COD value drops significantly. The smaller the COD value, the more conducive it is to degradation, thus reducing certain wastewater treatment costs.

[0102] 4. Add coagulant to the mixed solution and stir thoroughly. After stirring evenly, let it stand for 10-30 minutes to obtain a flocculated liquid. The reaction time is 5 minutes and the reaction temperature is 20°C. Filter the flocculated liquid to obtain a precipitate containing nickel and a purified liquid. Detect the fluorine (F) component and COD value in the purified liquid. The values ​​are shown in the following table:

[0103] Element Type F(mg / L) COD(mg / L) content 38.33 168

[0104] From the data in the table, it can be concluded that the recovery rate of fluorine is 96.7%, which is greater than 90%, and can effectively improve the recovery of hydrogen.

[0105] Example 3

[0106] According to the method provided in Example 1, the fluorine and COD recovery operation was actually performed on the sulfided liquid of the copper smelting process wastewater for the second time to confirm the recovery of fluorine and COD. The specific operation steps are as follows:

[0107] 1. Detect the fluorine (F) component and COD value in the sulfided copper smelting process wastewater. The values ​​are shown in the following table:

[0108] Element Type F(mg / L) COD(mg / L) content 1569 1236

[0109] 2. Calculate the dosage of potassium permanganate as follows:

[0110] The molar ratio of the amount of potassium permanganate added to the sodium fluorosilicate content in the copper smelting process wastewater after sulfidation is 3:1. Knowing the ratio of the molar mass of F in sodium fluorosilicate to the overall molar mass of sodium fluorosilicate, it can be known that the molar mass of sodium fluorosilicate (M_Na2SiF6) is 188.07 g / mol. Since the chemical formula of sodium fluorosilicate is Na2SiF6, the total molar mass ratio of F in sodium fluorosilicate is:

[0111] Ratio = 6*M(F) / M_Na2SiF6

[0112] =6*19.00 / 188.07

[0113] =114.00 / 188.07

[0114] =0.606 (approximately equal to)

[0115] Calculate the total content of sodium fluorosilicate:

[0116] m_Na2SiF6=F content / F ratio

[0117] =1569mg / L / 0.606

[0118] ≈2591.43mg / L

[0119] Calculate the amount of potassium permanganate required to react with it (n_KMnO4):

[0120] n_KMnO4=a*n_Na2SiF6

[0121] =3*(m_Na2SiF6 / M_Na2SiF6)

[0122] =3*(2591.43mg / L / 188.07g / mol)

[0123] ≈3*(2.59143g / L / 188.07g / mol)

[0124] ≈3*0.01377mol / L

[0125] ≈0.04131mol / L

[0126] Calculate the mass of potassium permanganate required (m_KMnO4):

[0127] m_KMnO4=n_KMnO4*M_KMnO4

[0128] =0.04131mol / L*158.04g / mol

[0129] ≈6.527 g / L;

[0130] 3. Add potassium permanganate at a ratio of 6.527 g / L to the sulfided liquid of copper smelting process wastewater, heat and stir, fully mix and react to obtain a mixed solution, the reaction temperature is 80°C, the reaction time is 6 hours, and the fluorine (F) component and COD value in the reaction solution are detected. The values ​​are shown in the following table:

[0131] Element Type F(mg / L) COD(mg / L) content 1506 320

[0132] From this table, we can know that after potassium permanganate reaction, COD value drops significantly. The smaller the COD value, the more conducive it is to degradation, thus reducing certain wastewater treatment costs.

[0133] 4. Add coagulant to the mixed solution and stir thoroughly. After stirring evenly, let it stand for 10-30 minutes to obtain a flocculated liquid. The reaction time is 3 minutes and the reaction temperature is 23°C. Filter the flocculated liquid to obtain a precipitate containing nickel and a purified liquid. Detect the fluorine (F) component and COD value in the purified liquid. The values ​​are shown in the following table:

[0134] Element Type F(mg / L) COD(mg / L) content 42.16 236

[0135] From the data in the table, it can be concluded that the recovery rate of fluorine is 97.2%, which is greater than 90%, and can effectively improve the recovery of hydrogen.

[0136] Example 4

[0137] According to the method provided in Example 1, the fluorine and COD recovery operation was actually performed on the sulfided liquid of the copper smelting process wastewater for the third time to confirm the recovery of fluorine and COD. The specific operation steps are as follows:

[0138] 1. Detect the fluorine (F) component and COD value in the sulfided copper smelting process wastewater. The values ​​are shown in the following table:

[0139] Element Type F(mg / L) COD(mg / L) content 1436 1238

[0140] 2. Calculate the dosage of potassium permanganate as follows:

[0141] 21. The molar ratio of the amount of potassium permanganate added to the sodium fluorosilicate content in the copper smelting process wastewater after sulfidation is 5:1. Knowing the ratio of the molar mass of F in sodium fluorosilicate to the overall molar mass of sodium fluorosilicate, it can be known that the molar mass of sodium fluorosilicate (M_Na2SiF6) is 188.07 g / mol. Since the chemical formula of sodium fluorosilicate is Na2SiF6, it can be seen that there are 6 F atoms in each molecule. Therefore, the total molar mass ratio of F in sodium fluorosilicate is:

[0142] Ratio = 6*M(F) / M_Na2SiF6

[0143] =6*19.00 / 188.07

[0144] =114.00 / 188.07

[0145] =0.606 (approximately equal to)

[0146] Calculate the total content of sodium fluorosilicate:

[0147] m_Na2SiF6=F content / F ratio

[0148] =1436mg / L / 0.606

[0149] ≈2371.54mg / L

[0150] Calculate the amount of potassium permanganate required to react with it (n_KMnO4):

[0151] n_KMnO4=a*n_Na2SiF6

[0152] =3*(m_Na2SiF6 / M_Na2SiF6)

[0153] =3*(2371.54mg / L / 188.07g / mol)

[0154] ≈3*(2.37154g / L / 188.07g / mol)

[0155] ≈3*0.01261mol / L

[0156] ≈0.03783mol / L

[0157] Calculate the mass of potassium permanganate required (m_KMnO4):

[0158] m_KMnO4=n_KMnO4*M_KMnO4

[0159] =0.03783mol / L*158.04g / mol

[0160] ≈5.987 g / L;

[0161] 3. Add potassium permanganate at a ratio of 5.987 g / L to the sulfided liquid of copper smelting process wastewater, heat and stir, fully mix and react to obtain a mixed solution. The reaction temperature is 100°C and the reaction time is 3 hours. Detect the fluorine (F) component and COD value in the reaction solution. The values ​​are shown in the following table:

[0162] Element Type F(mg / L) COD(mg / L) content 1324.9 306

[0163] From this table, we can know that after potassium permanganate reaction, COD value drops significantly. The smaller the COD value, the more conducive it is to degradation, thus reducing certain wastewater treatment costs.

[0164] 4. Add coagulant to the mixed solution and stir thoroughly. After stirring evenly, let it stand for 10-30 minutes to obtain a flocculated liquid. The reaction time is 1 minute and the reaction temperature is 25°C. Filter the flocculated liquid to obtain a precipitate containing nickel and a purified liquid. Detect the fluorine (F) component and COD value in the purified liquid. The values ​​are shown in the following table:

[0165] Element Type F(mg / L) COD(mg / L) content 33.12 276

[0166] From the data in the table, it can be concluded that the recovery rate of fluorine is 97.5%, which is greater than 90%, and can effectively improve the recovery of hydrogen.

[0167] In summary, the amount of potassium permanganate required for reacting with sodium fluorosilicate in the sulfided liquid of copper smelting process wastewater is first calculated, and then potassium permanganate is added to the sulfided liquid of copper smelting process wastewater for heating and stirring to obtain a mixed solution, and then a coagulant is added to the mixed solution for mixed stirring reaction to obtain a flocculated liquid, and finally the flocculated liquid is filtered to obtain a precipitate containing nickel and a purified liquid. The introduction of potassium permanganate promotes the transformation of sodium fluorosilicate, and the fluorine-containing compound is separated from the system in the form of precipitation. The newly generated sodium permanganate can effectively degrade the COD in the wastewater, improves the defluorination efficiency and depth, and also helps to degrade the COD to a certain extent, reduces a certain wastewater treatment cost, and reduces the calcium ion deposition and scaling in the defluorination process. The operation method of the present invention is simple, the process is simple and reliable, and it is easy to industrialize, and has important economic and social benefits.

[0168] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for removing fluorine and COD from sulfided copper smelting wastewater. Features: The steps include: S1. Calculate the amount of potassium permanganate required to react with sodium fluorosilicate based on the total content of sodium fluorosilicate in the sulfided copper smelting process wastewater; S2, adding potassium permanganate to the sulfided liquid of copper smelting process wastewater, heating and stirring, and fully mixing and reacting to obtain a mixed solution; S3, add a coagulant to the mixed solution and stir thoroughly, stir evenly and let stand for 10-30 minutes to obtain a flocculated solution; S4. Filter the flocculated liquid to obtain a precipitate containing nickel and a purified liquid.

2. A method for removing fluorine and COD from sulfided copper smelting wastewater according to claim 1, Features: In step S1, the amount of potassium permanganate is calculated as follows: A1. Determine the molar mass of sodium fluorosilicate (M_Na 2 SiF 6 ); A2. Calculate the amount of sodium fluorosilicate (n_Na) by dividing the total content of sodium fluorosilicate by the molar mass, with the total content in grams. 2 SiF 6 ); A3. According to the chemical reaction equation, determine the molar ratio of potassium permanganate to sodium fluorosilicate (a); A4. Calculate the amount of potassium permanganate required (n_KMnO 4 ): n_KMnO 4 =a*n_Na 2 SiF 6 ; A5. Determine the molar mass of potassium permanganate (M_KMnO 4 ); A6. Calculate the mass of potassium permanganate required (m_KMnO 4 ): m_KMnO 4 =n_KMnO 4 *M_KMnO 4 .

3. A method for removing fluorine and COD from sulfided copper smelting process wastewater according to claim 2, Features: In step S2, the molar ratio of the amount of potassium permanganate added to the amount of sodium fluorosilicate in the sulfided liquid of the copper smelting process wastewater is 1.5-5:

1.

4. A method for removing fluorine and COD from sulfided copper smelting wastewater according to claim 3, Features: The reaction conditions for adding potassium permanganate to the sulfided copper smelting process wastewater are as follows: the reaction temperature is 70-100° C. and the reaction time is 3-12 hours.

5. A method for removing fluorine and COD from sulfided copper smelting wastewater according to claim 4, Features: When the potassium permanganate reacts with the sulfided liquid of the copper smelting process wastewater, the potassium permanganate reacts with the organic matter in the wastewater to oxidize the organic matter into carbon dioxide and water.

6. A method for removing fluorine and COD from sulfided copper smelting wastewater according to claim 5, Features: In step S3, the coagulant aid is set to polyacrylamide with a molecular weight of 8 million to 18 million.

7. A method for removing fluorine and COD from sulfided copper smelting wastewater according to claim 6, Features: The mixed solution is added with a coagulant to carry out flocculation reaction. The amount of the coagulant added is 1-5 mL / (L·sulfurized liquid), the mass fraction of the coagulant is 0.1%-0.5%, and the conditions of the flocculation reaction are: reaction time is 1-5 min, and reaction temperature is 20-25° C.

8. A method for removing fluorine and COD from sulfided copper smelting wastewater according to claim 7, Features: When the coagulant is added, the coagulant is added to the mixed liquid by pumping, and then the mixed liquid is quickly stirred at a stirring rate of 400-800r / min using a stirring device to uniformly disperse the coagulant in the liquid. After stirring for 1-5 minutes, the stirring speed is reduced to 200-300r / min, and the mixed liquid is slowly stirred for 1-5 minutes. After the stirring is completed, the mixed liquid is allowed to stand for 10-30 minutes to allow the flocs to have enough time to settle to the bottom of the container.

9. A method for removing fluorine and COD from sulfided copper smelting wastewater according to claim 8, Features: In step S4, the precipitate needs to be subjected to nickel recovery, and the specific operation is as follows: B1, mixing the nickel-containing precipitate with a hydrochloric acid or nitric acid solution to dissolve the nickel and obtain a leaching solution; B2, filtering the leaching solution through a filtering device to obtain an insoluble residue and a clear liquid; B3, precipitating sodium hydroxide or potassium hydroxide in the clear solution to precipitate nickel as nickel hydroxide to obtain a precipitated nickel compound; B4. Calcine the precipitated nickel compound at high temperature to convert it into nickel oxide or metallic nickel.

10. A method for removing fluorine and COD from sulfided copper smelting wastewater according to claim 9, Features: The purified liquid needs to be purified, and the specific purification steps are as follows: C1. Use activated carbon filtering equipment to filter and remove organic matter, heavy metal ions or pigments in the solution to obtain a filtrate; C2. Perform reverse osmosis operation on the filtrate using a reverse osmosis device to remove dissolved solids and obtain reverse osmosis liquid; C3, sterilizing the reverse osmosis liquid through ultraviolet disinfection equipment to obtain treated liquid; C4: If the treated liquid meets the emission standards, it will be returned to the process for recycling. If the treated liquid does not meet the emission standards, it will be returned to C1.

Citation Information

Patent Citations

  • Method for recycling electrolytic zinc acid leaching slag

    CN102828033A

  • Method for treating fluosilicate waste residues

    CN104591223A

  • Method and system for recovering fluorine from waste acid produced in thinning production of solar cells or glass

    CN105753211A

  • Composite treatment agent for high-concentration ammonia nitrogen sewage and preparation method thereof

    CN117417061A

Cited By

  • Lead-bismuth smelting wastewater treatment method

    CN120309108A