Low-color-difference, self-cleaning and high-hardness coated glass and preparation method thereof

Through the combination of H-SiO2 nanoparticles and TiO2 sol and cationic polystyrene emulsion, low-color difference, self-cleaning, and high-hardness coating glass was prepared, which solved the problem of low mechanical strength and inconsistent color difference on the glass surface of photovoltaic modules, and achieved more High hardness and self-cleaning.

CN118930066APending Publication Date: 2024-11-12咸宁南玻玻璃有限公司 +1

Patent Information

Application Number
CN202411120069.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The glass surface of existing solar photovoltaic modules has problems of low mechanical strength and inconsistent color difference, making it difficult to achieve low color difference, high hardness and self-cleaning effects.

Method used

Using the combination of H-SiO2 nanoparticles and TiO2 sol and cationic polystyrene emulsion, low-chromatic, self-cleaning, and high-hardness coating glass was prepared by forming a core-shell silicon titanium sol and spraying, curing and tempering.

Benefits of technology

It improves the self-cleaning and hardness of the film surface, reduces the chromatic aberration, enhances the mechanical strength and adhesion of the glass, and meets the low chromatic aberration performance and high hardness requirements of photovoltaic modules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930066A_ABST
    Figure CN118930066A_ABST
Patent Text Reader

Abstract

The invention provides low-color-difference, self-cleaning and high-hardness coated glass and a preparation method thereof, and belongs to the technical field of glass processing. The hollow silica sol (HSiO2), the TiO2 sol and the cationic polystyrene emulsion are mixed, and a Ti-O-Si chemical bond is formed between the HSiO2 and the TiO2, so that the mechanical strength of the coating can be effectively improved, the pencil hardness of the film is improved, and the adhesive force between the glass substrates is further enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of glass processing, and relates to a low-color-difference, self-cleaning, high-hardness coated glass and a preparation method thereof. Background Art

[0002] The present invention is mainly used in the field of solar photovoltaic anti-reflection glass. The purpose is to provide a preparation of low-color difference, self-cleaning, high-hardness coated glass that is easy to apply or prepare. Due to the problems of fossil fuel consumption and environmental pollution, solar photovoltaic is becoming more and more important as a clean energy and renewable energy. If solar energy can be effectively utilized, the energy crisis can be solved to a certain extent. Solar modules have been installed to collect solar energy, and glass is widely used to protect active devices in the modules from harsh environments, such as wind and sandstorms. The wind blows dust and dirt onto the glass surface, covering the solar module, and these dust particles scatter light, preventing the incident light from reaching the solar cell; resulting in a decrease in output electrical power and a decrease in the utilization rate of solar energy. If the glass surface has a self-cleaning property, the adverse effects of subsequent pollutants on the light transmittance of the coating can be reduced.

[0003] However, conventional self-cleaning photovoltaic glass panels appear blue or light blue, and have low mechanical strength; they cannot meet customers' requirements for color consistency of the components and are not sufficient to prevent mechanical damage. Therefore, it is necessary to develop a film that can improve low color difference, achieve high hardness, and self-cleaning anti-reflection layer on the surface.

[0004] Existing technical problems:

[0005] (1) How to improve the low color difference performance of solar photovoltaic modules while achieving high hardness and surface self-cleaning.

[0006] (2) Production scale-up and processes that match the production workshop. Summary of the invention

[0007] The purpose of the present invention is to provide a low-color difference, self-cleaning, high-hardness coated glass and a preparation method in view of the above-mentioned problems existing in the prior art. The technical problem to be solved by the present invention is how to improve the low-color difference performance of solar photovoltaic modules while achieving high hardness and surface self-cleaning.

[0008] The object of the present invention can be achieved by the following technical scheme: A method for preparing low-color-difference, self-cleaning, high-hardness coated glass, comprising the following steps:

[0009] 1. Preparation of H-SiO2 nanoparticle sol

[0010] Take acrylic acid monomer and appropriate amount of initiator ammonium persulfate, emulsifier sodium dodecyl sulfate and deionized water and put them in the same four-necked bottle to prepare polyacrylic acid resin emulsion; mix appropriate amount of polyacrylic acid resin emulsion, silane, hydrochloric acid, anhydrous ethanol and isopropanol evenly, react at room temperature for 10 to 15 hours to prepare 50 to 200 nm H-SiO2 sol.

[0011] The acrylic monomer is one or more of acrylic acid, hydroxyethyl acrylate, methyl acrylate, ethyl acrylate, butyl acrylate, and methyl methacrylate;

[0012] The silane is one or more of orthosilicates, methylsiloxane, phenylsiloxane, vinylsiloxane, and acrylsiloxane.

[0013] 2. Preparation of TiO2 sol

[0014] Anhydrous ethanol, deionized water, hydrochloric acid and tetrabutyl titanate (TBOT) are placed in the same four-necked bottle and stirred at room temperature for 5 to 7 hours. The material is aged for 2 to 3 days and then diluted with a solvent to a solid content of 3 to 10%.

[0015] The above nEtOH:nH2O:nHCl:nTBOT=25:4:075:1;

[0016] The above solvent is one or more of anhydrous ethanol and isopropanol.

[0017] 3. Preparation of cationic polystyrene emulsion

[0018] Cationic polystyrene emulsion was prepared by referring to the methods in patents CN118126247A and CN105964195A.

[0019] 4. Preparation of coating solution

[0020] (1) doping the above-mentioned H-SiO2 sol, TiO2 sol and cationic polystyrene emulsion in proportion and mixing them with a solvent;

[0021] (2) adding silane to react for 5 to 24 hours at 10 to 40° C. to prepare a core-shell titanium-silicon sol;

[0022] (3) Add the core-shell titanium silicalite sol to a solvent and dilute the solid content to 3-5%.

[0023] The particle size of the cationic polystyrene emulsion is 50 to 200 nm;

[0024] The above-mentioned solvent is one or more of water, methanol, alcohol, isopropanol, ethylene glycol methyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, propylene glycol butyl ether, N,N-dimethylformamide, N,N-dimethylacetamide, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether, xylene, and cyclohexanone.

[0025] 5. Preparation of coated glass

[0026] The coating liquid is coated on the solar front panel glass by any coating method including spraying, dipping, pulling and rolling, and then cured at 100-200°C and tempered at 500-750°C to obtain low color difference, self-cleaning and high hardness coated glass.

[0027] The present invention uses a mixture of hollow silica sol (HSiO2), TiO2 sol and cationic polystyrene emulsion. The Ti-O-Si chemical bond formed between HSiO2 and TiO2 can effectively improve the mechanical strength of the coating, increase the pencil hardness of the film layer, and further enhance the adhesion between glass substrates.

[0028] The technical problem to be solved by the present invention is to invent a low-color difference, self-cleaning, high-hardness coated glass for photovoltaic modules and a preparation method thereof, so as to improve the self-cleaning property and hardness of the film surface and reduce the color difference.

[0029] 1) Provided are a low-color-difference, self-cleaning, high-hardness coated glass for photovoltaic modules and a preparation method thereof.

[0030] 2) Improve the quality of coated glass products. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is the measurement of film surface color difference.

[0032] Figure 2 This is a water contact angle test chart.

[0033] Figure 3 This is a pencil hardness test chart. DETAILED DESCRIPTION

[0034] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0035] The preparation of low-color-difference, self-cleaning, high-hardness coated glass for photovoltaic modules comprises the following steps:

[0036] 1. Preparation of H-SiO2 nanoparticle sol

[0037] Take acrylic acid monomer and appropriate amount of initiator ammonium persulfate, emulsifier sodium dodecyl sulfate and deionized water and put them in the same four-necked bottle to prepare polyacrylic acid resin emulsion; mix appropriate amount of polyacrylic acid resin emulsion, silane, hydrochloric acid, anhydrous ethanol and isopropanol evenly, react at room temperature for 10 to 15 hours to prepare 50 to 200 nm H-SiO2 sol.

[0038] The acrylic monomer is one or more of acrylic acid, hydroxyethyl acrylate, methyl acrylate, ethyl acrylate, butyl acrylate, and methyl methacrylate;

[0039] The silane is one or more of orthosilicates, methylsiloxane, phenylsiloxane, vinylsiloxane, and acrylsiloxane.

[0040] 2. Preparation of TiO2 sol

[0041] Anhydrous ethanol, deionized water, hydrochloric acid and tetrabutyl titanate (TBOT) are placed in the same four-necked bottle and stirred at room temperature for 5 to 7 hours. The material is aged for 2 to 3 days and then diluted with a solvent to a solid content of 3 to 10%.

[0042] The above nEtOH:nH2O:nHCl:nTBOT=25:4:075:1;

[0043] The above solvent is one or more of anhydrous ethanol and isopropanol.

[0044] 3. Preparation of cationic polystyrene emulsion

[0045] Cationic polystyrene emulsion was prepared by referring to the methods in patents CN118126247A and CN105964195A.

[0046] 4. Preparation of coating solution

[0047] (4) doping the above H-SiO2 sol, TiO2 sol and cationic polystyrene emulsion in proportion and mixing with a solvent;

[0048] (5) adding silane and reacting for 5 to 24 hours at 10 to 40° C. to prepare a core-shell titanium silicalite sol;

[0049] (6) Add the core-shell titanium silicalite sol to a solvent and dilute the solid content to 3-5%.

[0050] The particle size of the cationic polystyrene emulsion is 50 to 200 nm;

[0051] The above-mentioned solvent is one or more of water, methanol, alcohol, isopropanol, ethylene glycol methyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, propylene glycol butyl ether, N,N-dimethylformamide, N,N-dimethylacetamide, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether, xylene, and cyclohexanone.

[0052] 5. Preparation of coated glass

[0053] The coating liquid is coated on the solar front panel glass by any coating method including spraying, dipping, pulling and rolling, and then cured at 100-200°C and tempered at 500-750°C to obtain low color difference, self-cleaning and high hardness coated glass.

[0054] Performance Testing:

[0055] 1) Film color difference measurement: ΔE≤1.5, b: -2.5~0.5; colorless appearance; Figure 1 shown.

[0056] 2) Transmittance gain ≥ 2.3%, the curve has no obvious peaks, and no monochromatic light reflection;

[0057] 3) Water contact angle <10°, such as Figure 2 shown.

[0058] 4) Pencil hardness 9H, such as Figure 3 shown.

[0059] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A method for preparing low-color-difference, self-cleaning, high-hardness coated glass, characterized in that: The steps include: 1) Preparation of H-SiO2 nanoparticle sol Acrylic acid monomer, appropriate amount of initiator ammonium persulfate, emulsifier sodium dodecyl sulfate and deionized water are placed in the same four-necked bottle to prepare polyacrylic acid resin emulsion; appropriate amount of polyacrylic acid resin emulsion, silane, hydrochloric acid, anhydrous ethanol and isopropanol are mixed evenly, reacted at room temperature for 10 to 15 hours, and 50 to 200 nm H-SiO2 sol is prepared; 2) Preparation of TiO2 sol Put anhydrous ethanol, deionized water, hydrochloric acid and tetrabutyl titanate (TBOT) in the same four-necked bottle and stir at room temperature for 5-7 hours, age for 2-3 days, remove the material and dilute with solvent to 3-10% solid content; 3) Preparation of cationic polystyrene emulsion Cationic polystyrene emulsion was prepared by referring to the methods in patents CN118126247A and CN105964195A; 4) Preparation of coating solution (1) doping the above-mentioned H-SiO2 sol, TiO2 sol and cationic polystyrene emulsion in proportion and mixing them with a solvent; (2) adding silane to react for 5 to 24 hours at 10 to 40° C. to prepare a core-shell titanium-silicon sol; (3) adding a solvent to dilute the core-shell titanium silicalite sol to a solid content of 3 to 5%; 5) Preparation of coated glass The coating liquid is coated on the solar front panel glass by any coating method including spraying, dipping, pulling and rolling, and then cured at 100-200°C and tempered at 500-750°C to obtain low color difference, self-cleaning and high hardness coated glass.

2. The method for preparing low-color-difference, self-cleaning, high-hardness coated glass according to claim 1, characterized in that: The acrylic monomer in step 1) is one or more of acrylic acid, hydroxyethyl acrylate, methyl acrylate, ethyl acrylate, butyl acrylate, and methyl methacrylate.

3. The method for preparing low-color-difference, self-cleaning, high-hardness coated glass according to claim 1, characterized in that: The silane in step 1) is one or more of orthosilicates, methylsiloxane, phenylsiloxane, vinylsiloxane and acrylsiloxane.

4. The method for preparing low-color-difference, self-cleaning, high-hardness coated glass according to claim 1, characterized in that: In step 2), nEtOH:nH2O:nHCl:nTBOT=25:4:075:

1.

5. The method for preparing low-color-difference, self-cleaning, high-hardness coated glass according to claim 1, characterized in that: The solvent in step 2) is one or more of anhydrous ethanol and isopropanol.

6. The method for preparing low-color-difference, self-cleaning, high-hardness coated glass according to claim 1, characterized in that: The particle size of the cationic polystyrene emulsion in step 4) is 50 to 200 nm.

7. The method for preparing low-color-difference, self-cleaning, high-hardness coated glass according to claim 1, characterized in that: The solvent in step 4) is one or more of water, methanol, alcohol, isopropanol, ethylene glycol methyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, propylene glycol butyl ether, N,N-dimethylformamide, N,N-dimethylacetamide, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether, xylene, and cyclohexanone.

Citation Information

Patent Citations

  • Preparation method of modified organic silicon resin coating liquid and method for manufacturing solar battery packaging glass by using modified organic silicon resin coating liquid

    CN103555198A

  • Method for constructing self-cleaned anti-reflective film by using hollow nano composite particles

    CN104310791A

  • SiO2-TiO2 composite nanomaterial of core-shell structure and preparation method and application thereof

    CN104998629A

  • Method for preparing silicon dioxide / titanium dioxide composite film containing branch porous structure on substrate

    CN110272211A

  • Variable-refractive-index AG glass coating liquid and preparation method thereof, and method for manufacturing superhard AG coated glass

    CN112250315A

Cited By

  • Anti-deformation, anti-fading and anti-aging glass film and preparation method thereof

    CN120117844A