Unfired aggregate as well as preparation method and application thereof
Preparing burn-free aggregates by a mixture of solid waste powder and alkali slag, the problems of low strength and high temperature preparation of regenerated aggregates are solved, and high-strength and low-cost aggregates and water treatment filters are provided, which reduces concrete shrinkage and energy consumption, achieving the goals of solid waste absorption and environmental protection.
Patent Information
- Application Number
- CN202411158455.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
AI Technical Summary
The existing recycled aggregate has low strength, high temperature is required during the preparation process, and it cannot effectively alleviate the shortage of natural sand and gravel resources.
The mixture of solid waste powder and alkali residue is used to prepare burn-free aggregates through stirring and ball formation process to avoid high temperature treatment and form spherical particles, which are used for concrete and water treatment filter materials.
It provides high-strength and low-cost aggregate, reduces the shrinkage of concrete and mortar, and can be used as a water treatment filter material, with good bioadhesion and sewage interception capabilities, saves energy consumption and is environmentally friendly.
Smart Images

Figure BDA0005005748860000081
Abstract
Description
Technical Field
[0001] The invention provides a fire-free aggregate and a preparation method and application thereof, and relates to the technical field of comprehensive utilization of solid wastes. Background Art
[0002] Concrete is a commonly used man-made material in the construction industry. Its preparation uses sand and gravel as aggregates. Natural sand and gravel are obtained by digging rivers and mining mines, causing damage to the natural ecological environment. Sand and gravel are local materials and are not suitable for long-distance transportation. Natural sand and gravel resources have decreased in many areas. In order to reduce damage to the natural environment, studies have used lightweight aggregates, sintered ceramsite and recycled aggregates as concrete aggregates. During the setting and hardening process of concrete, the hydration of cementitious materials and changes in the external environmental conditions of concrete will cause concrete shrinkage, volume reduction, and then concrete cracking. Recycled aggregates can limit the volume shrinkage of concrete, but cannot alleviate the shrinkage cracking caused by capillary tension caused by internal water consumption and evaporation of cementitious materials. At the same time, its preparation requires high temperature and the steps are relatively cumbersome. The concrete prepared by it has low strength and high cost. It can only be used in a small number of special projects and cannot effectively alleviate the current situation of shortage of natural sand and gravel resources. Recycled aggregates have a single purpose and are generally only used for concrete preparation. Summary of the invention
[0003] The present invention provides a fire-free aggregate and a preparation method and application thereof, which solves the technical problems in the prior art that the strength of the recycled aggregate is low and the production steps require high temperatures.
[0004] The present invention is implemented in this way. The unburned aggregate includes the following components in parts by weight: 60 to 120 parts of solid waste powder, 0 to 40 parts of alkali slag, and 5 to 30 parts of water. The solid waste powder includes one or more of tailings powder, fly ash, desulfurized gypsum, Bayer red mud, brick slag powder, and coal gangue powder. The alkali slag includes one or more of calcium carbonate, calcium sulfate, calcium chloride, magnesium carbonate, sodium hydroxide, and calcium hydroxide.
[0005] As a further preferred embodiment, the specific surface area of the solid waste powder is 50 to 500 m 3 / kg.
[0006] The method for preparing the unburned aggregate comprises the following steps:
[0007] (1) stirring and mixing the solid waste powder and the alkali residue to obtain a first mixture;
[0008] (2) stirring and mixing the first mixture obtained in step (1) with water to obtain a second mixture;
[0009] (3) placing the second mixture into a spheronizer to form spherical particles;
[0010] (4) The spherical particles obtained in step (3) are sealed and cured.
[0011] As further preferred, the stirring and mixing conditions of step (1) are: rotation speed 90-150 r / min, time 1-3 min, temperature 0-40°C.
[0012] As further preferred, the stirring and mixing conditions of step (2) are: rotation speed 120-140 r / min, time 2.5-3 min, temperature 17-30°C.
[0013] As a further preference, the spherical particles obtained in step (3) have a particle size of 1 to 20 mm.
[0014] As a further preference, the sealing and curing conditions of step (4) are: temperature of 30-40° C. and time of 4-9 h.
[0015] Application of unburned aggregate, wherein the unburned aggregate is used as filter material for water treatment.
[0016] Beneficial effects of the present invention:
[0017] (1) The present invention provides unburned aggregates, the raw materials of which are solid waste and alkali slag, which are easy to obtain, low in price, and can also dispose of solid waste; the production process is simple, and high-temperature calcination and autoclave sealing maintenance are not required, which saves energy consumption and is low-carbon and environmentally friendly.
[0018] (2) The present invention provides a fire-free aggregate, which is non-toxic and pollution-free, has high strength, strong acid and alkali resistance, and has good adhesion to the cement stone interface, which can weaken or eliminate the weak link of the interface between natural aggregate and cement stone, and the prepared concrete and mortar have good workability. At the same time, it has high water absorption, releases water inside the concrete and mortar materials, reduces the autogenous stress of the concrete and mortar, and reduces or eliminates shrinkage.
[0019] (3) The unburned aggregate provided by the present invention can be used as a water treatment filter material and has good biological adhesion, biofilm formation performance and pollution interception ability. DETAILED DESCRIPTION
[0020] The technical solution of the present application is further described in detail below in conjunction with specific embodiments and experimental examples. The raw materials and equipment involved in the present application can be obtained commercially.
[0021] Example 1
[0022] A method for preparing a non-burning aggregate comprises the following steps:
[0023] (1) 55 parts by mass of tailings powder, 15 parts by mass of fly ash, 10 parts by mass of desulfurized gypsum, 5 parts by mass of Bayer red mud and 20 parts by mass of calcium carbonate were stirred and mixed to obtain a first mixture. The stirring conditions were: rotation speed 130 r / min, time 3 min, temperature 28°C.
[0024] (2) The first mixture obtained in step (1) was mixed with 20 parts by mass of water and stirred to obtain a second mixture. The stirring conditions were: rotation speed 120 r / min, time 2.5 min, temperature 30° C.
[0025] (3) The second mixture obtained in step (2) is placed in a spheronizer to obtain spherical particles with a particle size of 15 mm.
[0026] (4) The spherical particles obtained in step (3) are sealed and cured at 35° C. for 5 hours to obtain unburned aggregate.
[0027] Example 2
[0028] A method for preparing a non-burning aggregate comprises the following steps:
[0029] (1) 70 parts by mass of tailings powder, 25 parts by mass of fly ash, 10 parts by mass of desulfurized gypsum, 5 parts by mass of Bayer red mud, 15 parts by mass of calcium carbonate and 15 parts by mass of calcium sulfate were stirred and mixed to obtain a first mixture. The stirring conditions were: rotation speed 150 r / min, time 1 min, temperature 10°C.
[0030] (2) The first mixture obtained in step (1) was mixed with 20 parts by mass of water and stirred to obtain a second mixture. The stirring conditions were: rotation speed 130 r / min, time 3 min, temperature 30° C.
[0031] (3) The second mixture obtained in step (2) is placed in a spheronizer to obtain spherical particles with a particle size of 20 mm.
[0032] (4) The spherical particles of step (3) are sealed and cured at 25° C. for 5 hours to obtain unburned aggregate.
[0033] Example 3
[0034] A method for preparing a non-burning aggregate comprises the following steps:
[0035] (1) 70 parts by mass of tailings powder, 25 parts by mass of fly ash, 10 parts by mass of desulfurized gypsum, 5 parts by mass of Bayer red mud, 20 parts by mass of calcium sulfate, and 10 parts by mass of sodium hydroxide were stirred and mixed uniformly to obtain a first mixture. The stirring conditions were: a rotation speed of 150 r / min, a time of 1 min, and a temperature of 10°C.
[0036] (2) The first mixture obtained in step (1) was mixed with 20 parts by mass of water and stirred to obtain a second mixture. The stirring conditions were: rotation speed 130 r / min, time 3 min, temperature 30° C.
[0037] (3) The second mixture obtained in step (2) is placed in a spheronizer to obtain spherical particles with a particle size of 20 mm.
[0038] (4) The spherical particles of step (3) are sealed and cured at 25° C. for 5 hours to obtain unburned aggregate.
[0039] Example 4
[0040] A method for preparing a non-burning aggregate comprises the following steps:
[0041] (1) 55 parts by mass of tailings powder, 15 parts by mass of fly ash, 10 parts by mass of desulfurized gypsum, 15 parts by mass of calcium carbonate and 5 parts by mass of calcium hydroxide were mixed uniformly to obtain a first mixture. The stirring conditions were: a speed of 150 r / min, a time of 2 min, and a temperature of 20°C.
[0042] (2) The first mixture of step (1) was mixed with 20 parts by mass of water and stirred to obtain a second mixture. The stirring conditions were: rotation speed 120 r / min, time 3 min, temperature 17° C.
[0043] (3) The second mixture of step (2) is placed into a spheronizer to obtain spherical particles with a particle size of 10 mm.
[0044] (4) The spherical particles obtained in step (3) are sealed and cured at 30° C. for 9 hours to obtain a fire-free aggregate.
[0045] Example 5
[0046] A method for preparing a non-burning aggregate comprises the following steps:
[0047] (1) 53 parts by mass of tailings powder, 17 parts by mass of fly ash, 5 parts by mass of Bayer red mud, 15 parts by mass of coal gangue powder, 20 parts by mass of calcium sulfate and 5 parts by mass of calcium hydroxide were mixed uniformly to obtain a first mixture. The stirring conditions were: rotation speed 150 r / min, time 2 min, temperature 20°C.
[0048] (2) The first mixture of step (1) was mixed with 35 parts by mass of water and stirred to obtain a second mixture. The stirring conditions were: rotation speed 120 r / min, time 3 min, temperature 28° C.
[0049] (3) The second mixture obtained in step (2) is placed in a spheronizer to obtain spherical particles with a particle size of 20 mm.
[0050] (4) The spherical particles of step (3) are sealed and cured at 30° C. for 4 hours to obtain aggregate-free material.
[0051] Example 6
[0052] A method for preparing a non-burning aggregate comprises the following steps:
[0053] (1) 48 parts by mass of tailings powder, 10 parts by mass of desulfurized gypsum, 15 parts by mass of Bayer red mud, 10 parts by mass of coal gangue powder, 15 parts by mass of brick slag powder, 20 parts by mass of calcium chloride and 10 parts by mass of magnesium carbonate were mixed and stirred at a speed of 65 r / min, a time of 5 min and a temperature of 30° C. The mixture was stirred evenly to obtain a first mixture at a speed of 100 r / min, a time of 2 min and a temperature of 15° C.
[0054] (2) The first mixture obtained in step (1) was mixed with 30 parts by mass of water and stirred evenly under the stirring conditions of: rotation speed 120 r / min, time 3 min, temperature 22° C. to obtain a second mixture.
[0055] (3) The second mixture obtained in step (2) is placed in a spheronizer to obtain spherical particles with a particle size of 10 mm.
[0056] (4) The spherical particles obtained in step (3) are sealed and cured at 35° C. for 9 hours to obtain a fire-free aggregate.
[0057] Example 7
[0058] A method for preparing a non-burning aggregate comprises the following steps:
[0059] (1) 50 parts by mass of tailings powder, 17 parts by mass of fly ash, 10 parts by mass of desulfurized gypsum, 5 parts by mass of Bayer red mud, 10 parts by mass of coal gangue powder, 10 parts by mass of brick slag powder, 20 parts by mass of calcium carbonate and 20 parts by mass of magnesium carbonate were mixed uniformly to obtain a first mixture. The stirring conditions were: rotation speed 130 r / min, time 2 min, temperature 30°C.
[0060] (2) The first mixture obtained in step (1) was mixed with 10 parts by mass of water and stirred to obtain a second mixture. The stirring conditions were: a speed of 128 r / min, a time of 3 min, and a temperature of 26° C. to obtain a second mixture.
[0061] (3) The second mixture obtained in step (2) is placed in a spheronizer to obtain spherical particles with a particle size of 15 mm.
[0062] (4) The spherical particles of step (3) are sealed and cured at 30° C. for 6 hours to obtain unburned aggregate.
[0063] Example 8
[0064] A method for preparing a non-burning aggregate comprises the following steps:
[0065] (1) 60 parts by mass of tailings powder, 20 parts by mass of fly ash, 20 parts by mass of desulfurized gypsum, and 10 parts by mass of Bayer red mud were mixed and stirred to obtain a first mixture. The stirring conditions were: a speed of 140 r / min, a time of 2 min, and a temperature of 28° C.
[0066] (2) The first mixture obtained in step (1) was mixed with 40 parts by mass of water and stirred to obtain a second mixture. The stirring conditions were: rotation speed 135 r / min, time 3 min, temperature 28° C.
[0067] (3) The second mixture obtained in step (2) is placed in a spheronizer to obtain spherical particles with a particle size of 1 mm.
[0068] (4) The spherical particles obtained in step (3) are sealed and cured at 40° C. for 4 hours to obtain a fire-free aggregate.
[0069] Example 9
[0070] A method for preparing a non-burning aggregate comprises the following steps:
[0071] (1) 70 parts by mass of tailings powder, 25 parts by mass of fly ash, 10 parts by mass of Bayer red mud, 15 parts by mass of brick slag powder and 15 parts by mass of magnesium sulfate were mixed and stirred to obtain a first mixture. The stirring conditions were: a speed of 140 r / min, a time of 3 min, and a temperature of 28° C.
[0072] (2) The first mixture obtained in step (1) was mixed with 30 parts by mass of water and stirred to obtain a second mixture. The stirring conditions were: rotation speed 125 r / min, time 3 min, and temperature 28° C.
[0073] (3) The second mixture obtained in step (2) is placed in a spheronizer to obtain spherical particles with a particle size of 25 mm.
[0074] (4) The spherical particles obtained in step (3) are sealed and cured at 35° C. for 5 hours to obtain a fire-free aggregate.
[0075] Example 10
[0076] A method for preparing a non-burning aggregate comprises the following steps:
[0077] (1) 56 parts by mass of tailings powder, 19 parts by mass of fly ash, 10 parts by mass of desulfurized gypsum, 5 parts by mass of coal gangue powder and 30 parts by mass of calcium sulfate were mixed uniformly to obtain a first mixture. The stirring conditions were: rotation speed 125 r / min, time 2 min, temperature 35°C.
[0078] (2) The first mixture obtained in step (1) was mixed with 20 parts of water and stirred to obtain a second mixture. The stirring conditions were: rotation speed 120 r / min, time 3 min, temperature 17°C.
[0079] (3) The second mixture obtained in step (2) is placed in a spheronizer to obtain spherical particles with a particle size of 12 mm.
[0080] (4) The spherical particles obtained in step (4) are sealed and cured at 37° C. for 8 hours to obtain a fire-free aggregate.
[0081] Embodiment 11
[0082] A method for preparing a non-burning aggregate comprises the following steps:
[0083] (1) 40 parts by mass of tailings powder, 20 parts by mass of fly ash, 10 parts by mass of desulfurized gypsum, 5 parts by mass of Bayer red mud, 10 parts by mass of coal gangue powder, 15 parts by mass of brick slag powder and 20 parts by mass of calcium chloride were mixed and stirred to obtain a first mixture. The stirring conditions were: speed 140 r / min, time 3 min, temperature 40°C
[0084] (2) The first mixture obtained in step (1) was mixed with 20 parts by mass of water and stirred to obtain a second mixture. The stirring conditions were: rotation speed 125 r / min, time 3 min, temperature 20° C.
[0085] (3) The second mixture obtained in step (2) is placed in a spheronizer to obtain spherical particles with a particle size of 20 mm.
[0086] (4) The spherical particles are sealed and cured at 32°C for 6 hours to obtain unburned aggregate.
[0087] Example 12
[0088] A method for preparing a non-burning aggregate comprises the following steps:
[0089] (1) 84 parts by mass of tailings powder and 11 parts by mass of calcium carbonate were mixed uniformly to obtain a first mixture. The stirring conditions were: a speed of 150 r / min, a time of 2 min, and a temperature of 24° C.
[0090] (2) The first mixture of step (1) was mixed with 20 parts by weight of water and stirred to obtain a second mixture. The stirring conditions were: rotation speed 140 r / min, time 3 min, temperature 25° C.
[0091] (3) The second mixture obtained in step (2) is placed in a spheronizer to obtain spherical particles with a particle size of 7 mm.
[0092] (4) The spherical particles obtained in step (3) are sealed and cured at 35° C. for 4 hours to obtain a fire-free aggregate.
[0093] Embodiment 13
[0094] A method for preparing a non-burning aggregate comprises the following steps:
[0095] (1) 80 parts by mass of fly ash and 20 parts by mass of desulfurized gypsum were mixed and stirred evenly to obtain a first mixture. The stirring conditions were: rotation speed 100 r / min, time 3 min, temperature 30°C.
[0096] (2) The first mixture obtained in step (1) was mixed with 30 parts by mass of water and stirred to obtain a second mixture. The stirring conditions were: rotation speed 140 r / min, time 3 min, and temperature 20° C.
[0097] (3) The second mixture obtained in step (2) is placed in a spheronizer to obtain spherical particles with a particle size of 21 mm.
[0098] (4) The spherical particles obtained in step (3) are sealed and cured at 30° C. for 5 hours to obtain a fire-free aggregate.
[0099] Embodiment 14
[0100] A method for preparing a non-burning aggregate comprises the following steps:
[0101] (1) 80 parts by mass of Bayer red mud, 20 parts by mass of brick slag powder, 10 parts by mass of calcium chloride and 15 parts by mass of magnesium sulfate were mixed and stirred evenly to obtain a first mixture. The stirring conditions were: speed 130 r / min, time 3 min, temperature 28°C
[0102] (2) The first mixture obtained in step (1) was mixed with 30 parts by weight of water, and stirred evenly to obtain a second mixture. The stirring conditions were: a speed of 120 r / min, a time of 3 min, and a temperature of 30° C.
[0103] (3) The second mixture obtained in step (1) is placed in a spheronizer to obtain spherical particles with a particle size of 15 mm.
[0104] (4) The spherical particles obtained in step (3) are sealed and cured at 35° C. for 5 hours to obtain a fire-free aggregate.
[0105] Embodiment 15
[0106] A method for preparing a non-burning aggregate comprises the following steps:
[0107] (1) 80 parts by mass of tailings powder and 30 parts by mass of water were directly mixed and stirred to obtain a second mixture. The stirring conditions were: a speed of 140 r / min, a time of 3 min, and a temperature of 20° C.
[0108] (2) The second mixture obtained in step (1) is placed in a spheronizer to obtain spherical particles with a particle size of 15 mm.
[0109] (3) The spherical particles obtained in step (2) are sealed and cured at 30° C. for 6 hours to obtain a fire-free aggregate.
[0110] Example 16
[0111] A method for preparing a non-burning aggregate comprises the following steps:
[0112] (1) 90 parts by mass of Bayer red mud and 30 parts by mass of water were mixed and stirred evenly to obtain a second mixture. The stirring conditions were: a rotation speed of 140 r / min, a time of 3 min, and a temperature of 20° C.
[0113] (2) The second mixture obtained in step (1) is placed into a spheronizer to obtain spherical particles with a particle size of 5 mm.
[0114] (3) The spherical particles obtained in step (2) are sealed and cured at 35° C. for 5 hours to obtain a fire-free aggregate.
[0115] Embodiment 17
[0116] A method for preparing a non-burning aggregate comprises the following steps:
[0117] (1) 100 parts by mass of fly ash slurry and 30 parts by mass of water were mixed uniformly to obtain a second mixture. The stirring conditions were: a rotation speed of 130 r / min, a time of 3 min, and a temperature of 25° C.
[0118] (2) The second mixture obtained in step (1) is placed into a spheronizer to obtain spherical particles with a particle size of 5 mm.
[0119] (3) The spherical particles obtained in step (2) are sealed and cured at 35° C. for 6 hours to obtain a fire-free aggregate.
[0120] Embodiment 18
[0121] A method for preparing a non-burning aggregate comprises the following steps:
[0122] (1) 80 parts by mass of fly ash, 20 parts by mass of desulfurized gypsum and 30 parts by mass of water were mixed uniformly to obtain a second mixture. The stirring conditions were: a rotation speed of 140 r / min, a time of 2.5 min, and a temperature of 26° C.
[0123] (2) The second mixture obtained in step (1) is placed into a spheronizer to obtain spherical particles with a particle size of 5 mm.
[0124] (3) The spherical particles obtained in step (2) are sealed and cured at 35° C. for 6 hours to obtain a fire-free aggregate.
[0125] The fly ash used in Examples 1 to 18 is the third-level fly ash discharged from a power plant. The pelletizing machine is an existing pelletizing machine.
[0126] Experimental Example 1
[0127] The bulk density, apparent density, cylinder compressive strength, water absorption and softening coefficient were tested with reference to GB / T 17431.2-2010 “Lightweight aggregate and its test methods Part 2: Test methods for lightweight aggregate”. The results are shown in Table 1.
[0128] Table 1 Test data of Example 1 to Example 18
[0129]
[0130] As can be seen from Table 1, the unburned aggregates prepared in Examples 1 to 17 have high cylinder pressure strength and high water absorption, and can be used as concrete aggregates or as water treatment filter materials. The bulk density and apparent density are small, and the comprehensive performance is good. At the same time, the production process uses solid waste and low-temperature maintenance, which has the advantages of solid waste disposal and energy conservation and emission reduction.
[0131] Experimental Example 2
[0132] After the unfired aggregate prepared in the example was demoulded after initial setting, an unconfined compression test was carried out to measure the relative strength of the sample. The results are shown in Table 2.
[0133] Table 2 Relative strength of the unburned aggregates prepared in Examples 1-18
[0134] Relative strength / % Relative strength / % Example 1 208.6 Example 10 225.9 Example 2 221.5 Embodiment 11 203.3 Example 3 220.7 Example 12 120.4 Example 4 225.3 Embodiment 13 119.6 Example 5 222.8 Embodiment 14 132.5 Example 6 237.9 Embodiment 15 115.8 Example 7 236.1 Example 16 108.4 Example 8 198.7 Embodiment 17 112.7 Example 9 204.2 Embodiment 18 116.5
[0135] Combining Example 1 and Example 2 and Table 1 and Table 2, it can be seen that the cylinder pressure strength and relative strength measured in Example 2 are greater than the cylinder pressure strength and relative strength measured in Example 1, indicating that when the tailings powder is increased and the fly ash is increased at the same time, it indicates that the increase of fly ash in an appropriate amount can fill the voids in the aggregate and form sufficient cementitious material.
[0136] Combining Example 2 and Example 3 and Table 1 and Table 2, it can be seen that the cylinder pressure strength and relative strength measured in Example 2 are close to the cylinder pressure strength and relative strength measured in Example 3. When the amount of tailings powder used is large, the cylinder pressure strength and relative strength of the aggregate are not much different by adding an appropriate amount of alkali slag.
[0137] Combining Examples 4 to 7, and Tables 1 and 2, it can be seen that when coal gangue powder and brick slag are added to the solid waste, the cylinder pressure strength and relative strength of the unburned aggregate will increase. When the unburned aggregate is used as a water treatment filter material, the filtration and adsorption effect is better.
[0138] Combining Example 12, Example 13, Example 16 and Example 17, and combining Table 1 and Table 2, it can be seen that the cylinder compressive strength of the unburned aggregate prepared by mixing only one type of solid waste with alkali slag is lower than the cylinder compressive strength of the unburned aggregate prepared by adding multiple types of solid waste.
[0139] Beneficial effects of the present invention:
[0140] (1) The present invention provides unburned aggregates, the raw materials of which are solid waste and alkali slag, which are easy to obtain, low in price, and can also dispose of solid waste; the production process is simple, and high-temperature calcination and autoclave sealing maintenance are not required, which saves energy consumption and is low-carbon and environmentally friendly.
[0141] (2) The present invention provides an unburned aggregate, which is non-toxic and pollution-free, has high strength, strong acid and alkali resistance, and has good adhesion to the cement stone interface, which can weaken or eliminate the weak link of the interface between natural aggregate and cement stone, and the prepared concrete and mortar have good workability. At the same time, it has high water absorption, releases water inside the concrete and mortar materials, reduces the autogenous stress of the concrete and mortar, and reduces shrinkage.
[0142] (3) The unburned aggregate provided by the present invention can be used as a water treatment filter material and has good biological adhesion, biofilm formation performance and pollution interception ability.
[0143] The specific embodiments of the present invention are merely explanations of the present application and are not limitations of the present application. After reading this specification, those skilled in the art may make modifications to the embodiments without any creative contribution as needed. However, as long as they are within the scope of the claims of the present application, they shall be protected by the patent law.
Claims
1. A fire-free aggregate, characterized in that: The unburned aggregate includes the following components in parts by weight: 60 to 120 parts of solid waste powder, 0 to 40 parts of alkali slag, and 5 to 30 parts of water. The solid waste powder includes one or more of tailings powder, fly ash, desulfurized gypsum, Bayer red mud, brick slag powder, and coal gangue powder. The alkali slag includes one or more of calcium carbonate, calcium sulfate, calcium chloride, magnesium carbonate, sodium hydroxide, and calcium hydroxide.
2. The unburned aggregate according to claim 1, characterized in that: The specific surface area of the solid waste powder is 50 to 500 m 3 / kg.
3. The method for preparing a non-burning aggregate according to claim 1, characterized in that: The steps include: (1) stirring and mixing the solid waste powder and the alkali residue to obtain a first mixture; (2) stirring and mixing the first mixture obtained in step (1) with water to obtain a second mixture; (3) placing the second mixture into a spheronizer to form spherical particles; (4) The spherical particles obtained in step (3) are sealed and cured.
4. The preparation method according to claim 3, characterized in that: The stirring and mixing conditions of step (1) are: rotation speed 90-150 r / min, time 1-3 min, temperature 0-40° C.
5. The preparation method according to claim 3, characterized in that: The stirring and mixing conditions of step (2) are: rotation speed 120-140 r / min, time 2.5-3 min, temperature 17-30° C.
6. The preparation method according to claim 3, characterized in that: The spherical particles obtained in step (3) have a particle size of 1 to 20 mm.
7. The preparation method according to claim 3, characterized in that: The sealing and curing conditions of step (4) are: temperature of 30-40° C. and time of 4-9 hours.
8. The use of the unburned aggregate according to claim 1, characterized in that: The unburned aggregate is used as filter material for water treatment.