Polymer capsule for mass concrete self-repairing and preparation method thereof

By using polymer capsules of modified graphene and highly absorbent resin in large volumes of concrete, the crack problem of concrete when temperature changes is solved, and the crack repair is achieved evenly cracked when heat is achieved, which extends the service life of the concrete and reduces the Maintenance cost.

CN118930118APending Publication Date: 2024-11-12ZHENGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411065965.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Large volume concrete is prone to cracks when temperature changes. The existing expansion agent can only fail after the initial effect and cannot effectively repair internal cracks. The traditional repair method is costly and untimely.

Method used

Develop a polymer capsule containing modified graphene and highly absorbent resin, through the use of modifiers and crosslinking agents, to ensure that the capsules break evenly when heated, release the capsule core material to repair cracks, and to modify graphite Ethylene improves thermal conductivity and dispersion.

Benefits of technology

It realizes effective crack repair in large volume concrete, extends the service life of concrete, reduces maintenance costs, and can be mass-produced in industry, and is highly environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004979360340000011
    Figure HDA0004979360340000011
Patent Text Reader

Abstract

The invention belongs to the technical field of concrete self-repairing, and particularly relates to a polymer capsule for mass concrete self-repairing and a preparation method thereof. The polymer capsule is prepared from the following raw materials: a capsule core material, a capsule wall material a, a capsule wall material b, a solubilizer, a modifier, a cross-linking agent, a pH regulator, an organic solvent and a proper amount of deionized water. The polymer capsule disclosed by the invention can be added into mass concrete, and can be uniformly heated and timely broken in the early-stage mass concrete concentrated heat release cracking danger period, so that a capsule core material is released, and cracks generated by a matrix are repaired.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete self-repairing, and specifically relates to a polymer capsule for self-repairing large-volume concrete and a preparation method thereof. Background Art

[0002] The main reason for cracks in concrete is the change in its volume, one of the most important factors being temperature. Most hydraulic concretes are large-volume concretes with a small surface coefficient, concentrated heat release from cement hydration, and a relatively serious internal hydration temperature rise (temperature up to 80°C or above). The temperature difference between the inside and outside causes tensile stress on the surface; when the temperature drops, the inside begins to shrink, but due to the constraints of external conditions, temperature stress (tensile stress) is generated inside. When the tensile stress is greater than the tensile strength of the concrete, cracks will occur on its surface or inside, and in severe cases, vertical through cracks may form. Cracks in large-volume hydraulic concrete buildings not only affect the beauty and operation of the building itself, but also bring potential risks to the entire project, shorten the life of the project, and even worse, cause serious accidents, causing serious losses to the country and the people. Therefore, preventing the occurrence of cracks in hydraulic concrete and repairing cracks to increase its service life have always been a topic of concern to the engineering community and researchers.

[0003] In the early stage, cracks were mainly repaired by passive means such as regular maintenance in order to improve the durability of concrete. This method not only has high maintenance costs in the later stage, but can only repair surface cracks. Potential cracks inside cannot be discovered and effectively repaired in time, which still poses a potential threat. At present, the more economical and effective method to improve the durability of hydraulic concrete is to add one or more expansion agents to it, but the disadvantage of this method is that it can only improve the durability of concrete in a certain period of time. For example, calcium sulfoaluminate concrete expansion agents are widely used at present. This type of expansion agent undergoes hydration reaction in the cement environment to generate expansion products - calcium sulfonate (AFt). The expansion stress generated during the generation of AFt can compensate for the shrinkage deformation of the concrete structure, so that the concrete produces a stable volume expansion to resist the early shrinkage stress and reduce the generation of internal cracks. However, it is an early expansion agent, and the expansion period mainly works in 3-14 days of the concrete curing age. After 14 days, the expansion is basically completed and the expansion agent no longer continues to work. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a polymer capsule for self-repairing of large-volume concrete and a preparation method thereof, wherein the polymer capsule can be awakened by heat in large-volume concrete to repair cracks.

[0005] The technical solution adopted by the present invention is:

[0006] A polymer capsule for self-repairing of large-volume concrete, wherein the raw materials used are, by weight: 10-30 parts of capsule core material, 0.05-0.2 parts of capsule wall material a, 10-20 parts of capsule wall material b, 0.1-0.4 parts of solubilizer, 0.05-0.2 parts of modifier, 1-3 parts of cross-linking agent, 3-6 parts of pH regulator, and 10-20 parts of organic solvent

[0007] And appropriate amount of deionized water.

[0008] The size of the polymer capsule for self-repairing of large-volume concrete is 5.0-15.0 mm.

[0009] The capsule core material is a polyacrylic acid super absorbent resin, the main chemical component of which is low cross-linked sodium polyacrylate accounting for 88%, and the molecular formula is -(C3H3NaO2) n -, water accounts for 8%-10%, and the particle size is 200-250 mesh, i.e. 0.058-0.074mm.

[0010] The capsule wall material a is graphene, with a carbon content greater than 95%, a single layer rate of 80%, a thickness of 100nm, 50 =7~10μm, D 90 =15~20μm, specific surface area 50~200m 2 / g.

[0011] The capsule wall material b is gelatin with a relative molecular mass of 50,000 to 100,000 and a freezing strength of 220 to 250.

[0012] The modifier is 1-pyrenebutyric acid (PBA), potassium permanganate (KMnO4) or sodium dodecyl sulfate (SDS), the purity of PBA and SDS is 97%, and the purity of KMnO4 is analytical grade.

[0013] The modifier is preferably 1-pyrenebutyric acid (PBA).

[0014] The solubilizing agent is N-methylpyrrolidone (NMP) or dimethyl sulfoxide (DMSO), and the purity is analytical grade.

[0015] The cross-linking agent is one or more of ammonium persulfate, formaldehyde and acetaldehyde, and the purity is analytical grade.

[0016] The pH regulator is one or more of sulfuric acid and hydrochloric acid, with a concentration of 1 mol / L. The organic solvent is anhydrous ethanol, with a purity of 99.9%.

[0017] A method for preparing a polymer capsule comprises the following steps:

[0018] 1) Weigh each raw material according to the proportion;

[0019] 2) mixing the capsule wall material a, the solubilizing agent and deionized water, stirring and dispersing to obtain a suspension;

[0020] 3) adding the modifier to the suspension obtained in step 2), stirring, dispersing, washing (washing with deionized water 3 times), filtering and drying to obtain a modified capsule wall material a;

[0021] 4) adding an organic solvent into deionized water (25° C., 30-100 parts) to prepare a 20-30% organic solvent solution;

[0022] 5) dispersing the capsule core material in an organic solvent solution to obtain liquid A;

[0023] 6) Adding capsule wall material b into liquid A and stirring to obtain liquid B;

[0024] 7) adding the modified capsule wall material a into deionized water (50-100 parts), stirring and dispersing, and obtaining a suspension of the modified capsule wall material a (concentration of 0.5-2.0 g / L);

[0025] 8) Add the modified capsule wall material a suspension into liquid B and stir to obtain liquid C;

[0026] 9) dissolving the crosslinking agent in deionized water (40-80 parts), then adding dropwise to solution C, heating and stirring to obtain solution D;

[0027] 10) Adjust the pH of solution D to 5-6 with a pH adjuster, and let it stand (at 25°C for 3-6 hours) to obtain a gel;

[0028] 11) The gel is extruded and molded (extruder aperture 3.0-10.0 mm), washed (washed twice with deionized water), dried, and finally collected to obtain polymer capsules for self-repairing of large-volume concrete.

[0029] In the step 2), the amount of deionized water used is 12-14 times that of the capsule wall material a.

[0030] The optimal mass ratio of capsule wall material a, solubilizer and deionized water in step 2) is 6:12:82.

[0031] When dispersing in step 2) or step 3), ultrasonic dispersion is performed at a frequency of 40±2 KHz for 60-80 min; when dispersing in step 7), ultrasonic dispersion is performed at a frequency of 40±2 KHz for 15-20 min.

[0032] The stirring in steps 2), 3) and 6) is performed at a speed of 500-1000 r / min, the stirring time in steps 2) and 3) is 60-80 min, and the stirring time in step 6) is 15-20 min; the stirring in steps 7) and 8) is performed at a speed of 100-200 r / min and the stirring time is 30-40 min.

[0033] The heating and stirring in step 9) is carried out in a water bath, the heating temperature is 60-80° C., the stirring speed is 400-600 r / min, and the stirring time is 40-80 min.

[0034] The drying temperature in step 3) is 50-60° C. and the drying time is 24-36 hours; the drying in step 11) is to place the mixture in a forced air drying oven at 40-60° C. and dry it for 10-24 hours.

[0035] Compared with the prior art, the beneficial technical effects of the present invention are:

[0036] 1. In the research of the present invention, the inventors found that although the thermal conductivity of graphene is very high, its dispersibility is very poor. When added to water or gelatin, it will aggregate and cannot be evenly dispersed in the polymer capsule wall. When heated, the polymer capsules with graphene aggregation can be broken, but the capsules with low graphene content or uneven graphene distribution cannot be completely broken, and microcracks cannot be effectively repaired. Therefore, in the field of self-repairing capsules, graphene oxide will be added, and graphene oxide can be evenly dispersed in water or gelatin. However, although its dispersibility is excellent, many defects are introduced into the interior during its oxidation process, which destroys the perfect crystal structure of graphene, resulting in obstruction of phonon transmission and serious decline in thermal conductivity, and the purpose of repairing the thermal rupture of the repair capsule cannot be well achieved. The present invention improves the hydrophilicity of graphene without substantially affecting its thermal conductivity by modifying graphene, so that it can be more evenly dispersed in the wall material while ensuring high thermal conductivity. The polymer capsules of the present invention can be added to large-volume concrete. In the early stage of the dangerous cracking period when the large-volume concrete releases heat intensively, the polymer capsules can be heated evenly and ruptured in time, thereby releasing the capsule core material. The cracks in the matrix are repaired through the reaction between the water absorption (water is the excess water in the concrete structure) / water release behavior of the capsule core and the unhydrated cement.

[0037] 2. The present invention uses gelatin as the main wall material, which is relatively brittle after drying. The addition of modified graphene with excellent flexibility reduces the brittleness of the shell to a certain extent and reduces the risk of leakage of the highly absorbent resin during stirring.

[0038] 3. In the process of preparing capsules, carboxyl groups are introduced into the graphene structure by graphene modified by 1-pyrenebutyric acid or potassium permanganate. By adjusting the pH value of the system, substitution reaction will occur between the carboxyl group and the amino group or hydroxyl group in gelatin, which can firmly fix the modified graphene in the wall material. The bonding degree between the graphene and the wall material is good, and the graphene is not easy to fall off during the drying process, and the thermal conductivity of the polymer capsule is more stable and reliable. Furthermore, the present invention realizes the crosslinking between the capsule core material and the capsule wall material through a crosslinking agent, so that the capsule wall and the capsule core are tightly bonded. The material has the advantages of being cheap and easy to obtain, and having low pollution, and can achieve safe and low-cost production.

[0039] 4. When 1-pyrenebutyric acid is selected as the modifier, the 1-pyrenebutyric acid molecules can be connected and modified with graphene through π-π interaction, and carboxyl groups are introduced on the graphene surface to increase its hydrophilicity. At the same time, since the effect is non-covalent, it will not destroy the crystal conjugated structure of graphene and will not affect its thermal conductivity. However, when potassium permanganate is selected, defects will be introduced into the oxidation process of graphene, which will affect the thermal conductivity of graphene.

[0040] 5. The shell structure of the polymer capsule for self-repair of large-volume concrete prepared by the present invention has a certain strength after curing and is not easy to break during the preparation of cement slurry, thereby preventing the core material from being exposed to water too early. When the temperature inside the cement stone rises, the shell layer can be broken in time to allow the core material to absorb water.

[0041] 6. The heat-awakening polymer capsules for self-repair of large-volume hydraulic concrete prepared by the present invention have a simple preparation process, can be mass-produced in industry, and are clean and environmentally friendly during the production process. During the preparation process, the size of the capsules can be controlled by controlling the aperture of the extruder. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 1 is a correlation diagram between the capsule breakage rate and temperature of Examples 1-7. DETAILED DESCRIPTION

[0043] The specific implementation modes of the present invention are described below in conjunction with examples. However, the following examples are only used to illustrate the present invention in detail and are not intended to limit the scope of the present invention in any way.

[0044] In the following embodiments,

[0045] The size of the polymer capsule for self-repairing of large-volume concrete is 5.0-15.0 mm.

[0046] The main chemical component of polyacrylic acid super absorbent resin is low cross-linked sodium polyacrylate, accounting for 88%, and the molecular formula is -(C3H3NaO2) n-, water accounts for 8%-10%, and the particle size is 200-250 mesh, i.e. 0.058-0.074mm.

[0047] The carbon content of graphene is greater than 95%, the monolayer rate is 80%, the thickness is 100nm, D 50 =7~10μm, D 90 =15~20μm, specific surface area 50~200m 2 / g.

[0048] The relative molecular mass of gelatin is 50,000 to 100,000, and the freezing strength is 220 to 250.

[0049] The purity of 1-pyrenebutyric acid PBA and sodium dodecyl sulfate SDS is 97%, and the purity of potassium permanganate KMnO4 is analytical grade.

[0050] The purity of N-methylpyrrolidone (NMP) or dimethyl sulfoxide (DMSO) was analytical grade.

[0051] Ammonium persulfate, formaldehyde, and acetaldehyde were of analytical grade.

[0052] The concentration of sulfuric acid and hydrochloric acid is 1 mol / L; the purity of anhydrous ethanol is 99.9%.

[0053] Embodiment 1:

[0054] A polymer capsule comprises the following raw materials: 200 g of polyacrylic acid superabsorbent resin, 100 g of gelatin, 20 g of ammonium persulfate, 100 g of anhydrous ethanol and deionized water.

[0055] Preparation process:

[0056] 1) Take each raw material according to the amount;

[0057] 2) Add anhydrous ethanol to 500 g of deionized water at 25° C. and mix well to prepare a 20% anhydrous ethanol solution;

[0058] 3) dispersing the polyacrylic acid super absorbent resin in the anhydrous ethanol solution obtained in step 2) at 25° C. to obtain liquid A;

[0059] 4) Add gelatin to solution A and stir at 100 r / min for 30 min to obtain solution B;

[0060] 5) Dissolve ammonium persulfate in 400 g of deionized water, then slowly add it dropwise to solution B, heat in a water bath at 70°C, and stir at 500 r / min for 50 min to obtain gel A;

[0061] 6) Gel A was dropped into a watch glass via a syringe (aperture 6 mm), washed twice with deionized water, placed in a forced air drying oven at 40° C. for 24 h, and finally polymer capsules (5-10 mm) were collected.

[0062] Example 2

[0063] A polymer capsule comprises the following raw materials: 200 g of polyacrylic acid superabsorbent resin, 1 g of graphene, 100 g of gelatin, 20 g of ammonium persulfate, 100 g of anhydrous ethanol and deionized water.

[0064] Preparation process:

[0065] 1) Take each raw material according to the amount;

[0066] 2) Add anhydrous ethanol to 500 g of deionized water at 25° C. and mix well to prepare a 20% anhydrous ethanol solution;

[0067] 3) dispersing the polyacrylic acid super absorbent resin in the anhydrous ethanol solution obtained in step 2) at 25° C. to obtain liquid A;

[0068] 4) adding graphene to deionized water, stirring, and ultrasonically dispersing at a frequency of 40 KHz for 20 min to obtain a graphene suspension with a concentration of 1.0 g / L;

[0069] 5) Add gelatin to solution A and stir at 100 r / min for 30 min to obtain solution B;

[0070] 6) Add the graphene suspension to solution B and stir to obtain solution C;

[0071] 7) Dissolve ammonium persulfate in 400 g of deionized water, then slowly add it dropwise to solution C, heat in a 70°C water bath, stir at 500 rpm for 50 min to obtain solution D, and let solution D stand at 25°C for 6 h to obtain gel A;

[0072] 8) Gel A was dropped into a watch glass via a syringe (aperture 6 mm), washed twice with deionized water, placed in a forced air drying oven at 40° C. for 24 h, and finally polymer capsules (5-10 mm) were collected.

[0073] Example 3

[0074] A polymer capsule for self-repairing of large-volume concrete. The raw materials used are: 200 g of polyacrylic acid superabsorbent resin, 1 g of graphene, 100 g of gelatin, 2 g of N-methylpyrrolidone, 1 g of 1-pyrenebutyric acid, 20 g of ammonium persulfate, 40 g of sulfuric acid, 100 g of anhydrous ethanol and deionized water.

[0075] Preparation process:

[0076] 1) Take each raw material according to the amount;

[0077] 2) mixing graphene, N-methylpyrrolidone and 14 g of deionized water, and ultrasonically dispersing at a frequency of 40 KHz for 60 min to obtain a graphene suspension;

[0078] 3) adding 1-pyrenebutyric acid to the graphene suspension, stirring, ultrasonically dispersing at a frequency of 40 KHz for 60 min, washing with deionized water for 3 times, filtering, and drying to obtain modified graphene;

[0079] 4) Add anhydrous ethanol to 500 g of deionized water at 25° C. and mix well to prepare a 20% anhydrous ethanol solution;

[0080] 5) dispersing the polyacrylic acid super absorbent resin in the anhydrous ethanol solution obtained in step 2) at 25° C. to obtain liquid A;

[0081] 6) adding the modified graphene obtained in step 3) into deionized water, stirring, and ultrasonically dispersing at a frequency of 40 KHz for 20 min to obtain a modified graphene suspension with a concentration of 1.0 g / L;

[0082] 7) Add gelatin to solution A and stir at 100 r / min for 30 min to obtain solution B;

[0083] 8) adding the modified graphene suspension obtained in step 6) to liquid B and stirring to obtain liquid C containing modified graphene;

[0084] 9) Dissolve ammonium persulfate in 400 g of deionized water, then slowly add it dropwise to solution C, heat in a 70°C water bath, and stir at 500 rpm for 50 min to obtain solution D;

[0085] 10) adding sulfuric acid to solution D to adjust the pH to 5-6 to obtain solution E, and placing solution E at 25° C. for 5 h to obtain gel A;

[0086] 11) Gel A was dropped into a watch glass via a syringe (aperture 6 mm), washed twice with deionized water, placed in a forced air drying oven at 40° C. for 24 h, and finally polymer capsules (5-10 mm) were collected.

[0087] Example 4

[0088] A polymer capsule for self-repairing of large-volume concrete. The raw materials used are: 200 g of polyacrylic acid superabsorbent resin, 1 g of graphene, 100 g of gelatin, 2 g of N-methylpyrrolidone, 1 g of potassium permanganate, 20 g of ammonium persulfate, 40 g of sulfuric acid, 100 g of anhydrous ethanol and deionized water.

[0089] The preparation process was similar to that of Example 3, except that the modifier was replaced with potassium permanganate, and the resulting polymer capsules were 5-10 mm.

[0090] Example 5

[0091] A polymer capsule for self-repairing of large-volume concrete. The raw materials used are: 200 g of polyacrylic acid superabsorbent resin, 1 g of graphene, 100 g of gelatin, 2 g of N-methylpyrrolidone, 1 g of sodium dodecyl sulfate, 20 g of ammonium persulfate, 40 g of sulfuric acid, 100 g of anhydrous ethanol and deionized water.

[0092] The preparation process was similar to that of Example 3, except that the modifier was replaced with sodium dodecyl sulfate, and the resulting polymer capsules were 5-10 mm.

[0093] Example 6

[0094] A polymer capsule for self-repairing of large-volume concrete, the raw materials used are: 200g of polyacrylic acid superabsorbent resin, 1g of graphene, 100g of gelatin, 2g of N-methylpyrrolidone, 1g of 1-pyrenebutyric acid, 20g of ammonium persulfate, 100g of anhydrous ethanol and deionized water.

[0095] The difference from Example 3 is that the pH value of solution D is not adjusted, but it is directly allowed to stand at 25° C. for 6 hours to obtain gel A. The other steps are the same as those of Example 3, and the obtained polymer capsules are 5-10 mm.

[0096] Example 7

[0097] A polymer capsule for self-repairing of large-volume concrete. The raw materials used are: 100 g of polyacrylic acid superabsorbent resin, 2 g of graphene, 200 g of gelatin, 4 g of N-methylpyrrolidone, 2 g of 1-pyrenebutyric acid, 30 g of ammonium persulfate, 60 g of sulfuric acid, 200 g of anhydrous ethanol and deionized water.

[0098] Preparation process:

[0099] 1) Take each raw material according to the amount;

[0100] 2) mixing graphene, N-methylpyrrolidone and 24 g of deionized water, and ultrasonically dispersing at a frequency of 42 KHz for 80 min to obtain a graphene suspension;

[0101] 3) adding 1-pyrenebutyric acid to the graphene suspension, stirring, and ultrasonically dispersing at a frequency of 42 kHz for 80 min, washing with deionized water for 3 times, filtering, and drying to obtain modified graphene;

[0102] 4) adding anhydrous ethanol to deionized water at 25° C. and mixing well to prepare a 20% anhydrous ethanol solution;

[0103] 5) dispersing the polyacrylic acid super absorbent resin in the anhydrous ethanol solution obtained in step 2) at 25° C. to obtain liquid A;

[0104] 6) adding the modified graphene obtained in step 3) into deionized water, stirring, and ultrasonically dispersing at a frequency of 42 kHz for 15 min to obtain a modified graphene suspension with a concentration of 1.0 g / L;

[0105] 7) Add gelatin to solution A and stir at 100 r / min for 30 min to obtain solution B;

[0106] 8) adding the modified graphene suspension obtained in step 6) to liquid B and stirring to obtain liquid C containing modified graphene;

[0107] 9) Dissolve ammonium persulfate in 600 g of deionized water, then slowly add it dropwise to solution C, heat in a water bath at 80°C, and stir at 400 r / min for 80 min to obtain solution D;

[0108] 10) adding sulfuric acid to solution D to adjust the pH to 5-6 to obtain solution E, and placing solution E at 25° C. for 5 h to obtain gel A;

[0109] 11) Gel A was dropped into a watch glass via a syringe (aperture 10 mm), washed twice with deionized water, placed in a forced air drying oven at 60° C. for 15 h, and finally polymer capsules (10-15 mm) were collected.

[0110] Effect experiment 1:

[0111] Simulate the effect of temperature rise on the breakage rate of capsules. During the experiment, the capsules prepared in Examples 1-7 were placed in water of different temperatures to simulate the temperature at different locations in a large volume of concrete and explore the effect of ambient temperature on the breakage rate of capsules. Figure 1 shown.

[0112] Depend on Figure 1It can be seen that the crushing rate of each group of capsules will gradually increase with the increase of temperature, but there are differences in the crushing effects between different embodiments. By comparing Examples 1, 2 and 3, it can be found that the crushing effects of Examples 2 and 3 are better than those of Example 1, indicating that the introduction of graphene and modified graphene has increased the crushing rate of the capsules. However, the capsules of Example 2 began to break in large quantities at temperatures above 60°C, and the final crushing rate was about 90%, while the capsules of Example 3 began to break in large quantities at temperatures above 40°C, and the crushing rate reached 100% at 60°C, and there was a linear correlation between the crushing rate and the temperature change. The reason is that it is directly related to the dispersibility of graphene in gelatin and the degree of bonding between graphene and gelatin. When graphene is unevenly dispersed, the wall materials of some capsules contain little or no graphene, and the thermal conductivity of these capsules will be affected, and the capsules will not reach the temperature of rupture. The unmodified graphene in Example 2 is prone to aggregation, resulting in uneven dispersion in gelatin. At this time, the graphene and gelatin are physically adhered, and this physical adhesion is not stable. After the graphene in Example 3 is modified by 1-pyrenebutyric acid π-π interaction, carboxyl groups are introduced into the surface of the graphite gap, and the hydrophilicity is enhanced; at the same time, the introduced carboxyl groups react with the amino groups or hydroxyl groups in the gelatin in an acidic environment. The modified graphene in Example 3 can be evenly dispersed in the gel, and can form a whole with gelatin and SAP through non-covalent or covalent interactions, making its thermal conductivity more stable and reliable.

[0113] Comparative Examples 3, 4 and 5 show that different modifiers have a greater impact on the thermal conductivity and dispersibility of graphene. When graphene is modified with potassium permanganate, although the dispersibility of graphene is improved, a large number of defects are introduced during the oxidation process, destroying the graphene crystal sheet structure, which hinders the propagation of phonons and reduces the thermal conductivity. When graphene is modified with sodium dodecyl sulfate, although the thermal conductivity of graphene is less damaged, since SDS can only be adsorbed on the graphene surface through a physical adsorption process, and its adsorption process is affected by the number of graphene layers, etc., the dispersion ability of graphene is limited, resulting in the capsule breakage rate of Example 5 being not as good as that of Example 3. The comparison of Examples 3 and 6 further verifies the influence of the degree of bonding between modified graphene and the capsule wall material on the uniformity of thermal rupture of the capsule. The comparison of Examples 3 and 7 shows that the change in the relative amount of capsule core and capsule wall within a certain range has little effect on the capsule breakage rate.

[0114] Effect experiment 2:

[0115] Prefabricated 100×100×400mm 3The concrete test blocks were cured by electric heating to simulate the internal temperature environment of large-volume concrete, with three replicates in each group. The cement was PO42.5 cement, the sand was standard sand, the water-cement ratio was 0.50, the conductive carbon fiber was 1 vol% (accounting for the volume of the cementitious material), and the polymer capsule dosage was set to 1 wt.%. First, the cement, conductive carbon fiber and water were poured into a stirring pot and stirred slowly for 2 minutes, stopped for 15 seconds, and stirred quickly for 2 minutes; then the standard sand was poured into the stirring pot and stirred quickly for 2 minutes; finally, the polymer capsule was added and stirred slowly for 1 minute to obtain the polymer capsule mortar. The prepared mortar was poured into the mold (a conductive wire mesh was inserted at 100 mm from the edge during the pouring process), and the mold was removed after curing for 1 day at a temperature of 25°C, a relative humidity of 60%, and a voltage of 100V to 60°C. The test block was then cured for 28 days with a voltage of 100V. The flexural strength of the block was tested first, and then the compressive strength of the test block was tested. The average compressive strength and average flexural strength of each group were calculated. The two control groups Z0 and Z0-room were also cured for 28 days with a voltage of 100V and without voltage, respectively, and their compressive and flexural strengths were measured to explore the effect of the capsule on the self-healing effect. The experimental arrangement and experimental results are as follows:

[0116] Table 1 Experimental arrangement of capsule types on concrete self-repairing effect

[0117] serial number P.O42.5(g) Standard sand(g) Water(g) Capsule Type Z0-Room 2250 6750 1125 - Z0 2250 6750 1125 - Z1 2250 6750 1125+225 Example 1 Z2 2250 6750 1125 Example 2 Z3 2250 6750 1125 Example 3 Z4 2250 6750 1125 Example 4 Z5 2250 6750 1125 Example 5 Z6 2250 6750 1125 Example 6 Z7 2250 6750 1125 Example 7

[0118] Table 2 Effect of capsule types on concrete self-repairing in application examples

[0119] serial number Compressive strength(MPa) Flexural strength(MPa) Compressive strength residual rate (%) Residual rate of flexural strength (%) Z0-Room 45.5 12.5 - - Z0 27.7 8.5 60.9 68.0 Z1 26.9 8.0 59.2 64.0 Z2 31.9 9.4 70.2 75.5 Z3 43.4 11.8 95.5 94.2 Z4 38.9 10.4 85.5 83.1 Z5 36.4 9.6 80.0 76.9 Z6 41.4 11.5 91.1 89.2 Z7 42.1 11.6 92.5 92.4

[0120] As can be seen from the Z1 group in Table 1, the capsules prepared in Example 1 require additional water to ensure the stirring of the slurry. This is because the capsules prepared in Example 1 are relatively brittle, and more ruptures occur during the stirring process, and the SAP releases and absorbs water. The other groups do not require additional water, which shows the advantage of introducing graphene with excellent flexibility into the capsule wall.

[0121] As shown in Table 2, the introduction of capsules will cause a certain decrease in the mechanical properties of the samples (the residual rate of compressive strength / flexural strength is less than 100%). This is because more interfaces appear in the test samples after the introduction of capsules. When the load is applied, the stress will be concentrated on the interface, thereby reducing the mechanical properties. Although the mechanical properties are reduced to a certain extent, they can still meet the actual needs (except for group Z1).

[0122] It was found from the Z0-room and Z0 that long-term electric heating curing will significantly reduce the mechanical properties of concrete, which is consistent with the situation of large-volume concrete, indicating that the test can be roughly simulated. The introduction of capsules can increase the residual rate of mechanical properties (except for group Z1), which is due to the repair effect of capsules. The larger the residual rate of mechanical properties, the better the repair effect brought by the capsules. The residual rate is the best in group Z3, which also shows that the repair effect of the graphene group modified by 1-pyrenebutyric acid is the best.

[0123] Compared with Z1, it can be found that the graphene-containing capsules of Z2 and Z3 can greatly increase the residual rate of mechanical properties, indicating that some cracks have been repaired. This is mainly attributed to the fact that when the capsule breaks, the release of the capsule core material can break and repair the cracks in time. The higher the mechanical residual rate, the higher the repair rate. Comparing Z2 and Z3, it was found that the modified graphene has a better repair effect. This is because the Z3 capsule has better thermal rupture uniformity. The modified graphene in the Z3 capsule is more evenly distributed. Under the action of heat, it can be broken and the cracks can be repaired. However, the graphene in Z2 is unevenly dispersed. Some capsules may contain very little or no graphene. The thermal conductivity of these capsules is relatively poor, and they cannot break in time to achieve a repair effect, indicating that the thermal rupture uniformity of the Z2 capsule is not good.

[0124] Comparison of Z3, Z4 and Z5 revealed that different modification methods had different effects on the capsule loss rate. This was mainly attributed to the different modification methods causing different graphene dispersion uniformity or graphene thermal conductivity in the capsule, which in turn affected the uniformity of thermal rupture of the capsule, and affected the degree of rupture and repair of the capsule. Among them, the graphene group modified with 1-pyrenebutyric acid in group Z3 was the best.

[0125] Comparing Z3 and Z6, it was found that the mechanical residual rate of Z6 group was lower than that of Z3 group. The reason is related to the degree of bonding between graphene and the capsule wall. Without pH adjustment, the cross-linking between graphene and the capsule wall will be affected, and the degree of bonding between graphene and the capsule wall will also be affected. When graphene is firmly bonded to the capsule wall material, it is not easy for graphene to fall off during the preparation process. On the contrary, graphene will fall off during the preparation process. It can be seen that the degree of bonding between graphene and the capsule wall will also affect the repair effect.

[0126] By comparing Z3 and Z7, it was found that the change in the relative amount of the capsule core and the capsule wall within a certain range had little effect on the mechanical residual rate, and could also achieve a relatively ideal repair effect.

[0127] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in the field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.

[0128] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in the field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.

Claims

1. A polymer capsule for self-repair of large-volume concrete, It is characterized in that In parts by weight, the raw materials used are: 10-30 parts of capsule core material, 0.05-0.2 parts of capsule wall material a, 10-20 parts of capsule wall material b, 0.1-0.4 parts of solubilizer, 0.05-0.2 parts of modifier, 1-3 parts of cross-linking agent, 3-6 parts of pH adjuster, 10-20 parts of organic solvent and appropriate amount of deionized water.

2. The polymer capsule according to claim 1, Features: The size of the polymer capsule for self-repairing of large-volume concrete is 5.0-15.0 mm.

3. The polymer capsule according to claim 1, Features: The capsule core material is a polyacrylic acid superabsorbent resin, the capsule wall material a is graphene, and the capsule wall material b is gelatin.

4. The polymer capsule according to claim 1, Features: The modifier is 1-pyrenebutyric acid, potassium permanganate or sodium dodecyl sulfate; the solubilizer is N-methylpyrrolidone or dimethyl sulfoxide.

5. The polymer capsule according to claim 1, Features: The cross-linking agent is one or more of ammonium persulfate, formaldehyde, and acetaldehyde; the pH regulator is one or more of sulfuric acid and hydrochloric acid; and the organic solvent is anhydrous ethanol.

6. A method for preparing the polymer capsule according to claim 1, It is characterized in that The following steps are involved: 1) Weigh each raw material according to the proportion; 2) mixing the capsule wall material a, the solubilizing agent and deionized water, stirring and dispersing to obtain a suspension; 3) adding a modifier to the suspension obtained in step 2), stirring, dispersing, washing, filtering and drying to obtain a modified capsule wall material a; 4) adding an organic solvent into deionized water to prepare a 20-30% organic solvent solution; 5) dispersing the capsule core material in an organic solvent solution to obtain liquid A; 6) Add capsule wall material b into liquid A and stir to obtain liquid B; 7) adding the modified capsule wall material a into deionized water, stirring and dispersing, to obtain a suspension of the modified capsule wall material a; 8) Add the modified capsule wall material a suspension into liquid B and stir to obtain liquid C; 9) Dissolve the crosslinking agent in deionized water, then add dropwise to solution C, heat and stir to obtain solution D; 10) adjusting the pH of solution D to 5-6 with a pH adjuster, and allowing to stand to obtain a gel; 11) The gel is extruded into a shape, washed, dried, and finally collected to obtain polymer capsules for large-volume concrete self-repair.

7. The preparation method according to claim 6, Features: In the step 2), the amount of deionized water used is 12-14 times that of the capsule wall material a.

8. The preparation method according to claim 6, Features: When dispersing in step 2) or step 3), ultrasonic dispersion is performed at a frequency of 40±2 KHz for 60-80 min; when dispersing in step 7), ultrasonic dispersion is performed at a frequency of 40±2 KHz for 15-20 min.

9. The preparation method according to claim 6, Features: The stirring in steps 2), 3) and 6) is performed at a speed of 500-1000 r / min, the stirring time in steps 2) and 3) is 60-80 min, and the stirring time in step 6) is 15-20 min; the stirring in steps 7) and 8) is performed at a speed of 100-200 r / min and the stirring time is 30-40 min.