High-strength mineral composite casting formula and production and preparation process thereof
By using specific formulas and process treatments in mineral castings, mineral composite castings with high binding strength are formed, which solves the problem of low mechanical strength of mineral castings, improves their crack and peel resistance, and is suitable for high-precision parts processing.
Patent Information
- Application Number
- CN202310516934.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-12
AI Technical Summary
Mineral castings have low mechanical strength and are prone to cracking and breaking, and the broken grains are mainly concentrated in the bonding interface between resin and stone, resulting in the bonding interface being completely peeled off from the surface of the stone.
Pretreated granite, bisphenol A type phenolic epoxy resin prepolymer, bisphenol F type benzoxazine, N-aminoethylpiperazine, titanium tetrachloride, corundum powder, non-floating aluminum powder, aramid Materials such as fiber and sepiolite form an IPN resin interface between granite aggregate with microscopic fissures and pores and spatial hinge network structure through specific mixing and heating treatment to improve binding strength.
The formation of mineral composite castings with high bond strength reduces interface peeling and improves mechanical strength, and is suitable for high-precision parts processing.
Smart Images

Figure CN118930129A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite mineral castings, in particular to a high-strength mineral composite casting formula and a production and preparation process thereof. Background Art
[0002] Machine tools (Lathe) are equipment that mainly use turning tools to turn rotating workpieces. Drills, reamers, reamers, taps, dies and knurling tools can also be used on machine tools for corresponding processing. Some parts with high processing precision requirements need to be cut and finished on machine tools. The stricter the precision requirements of the processed parts, the higher the requirements for the stability and shock absorption of the machine tool bed.
[0003] Composite materials have a deeper development potential than single materials. With the development of science and technology, single metal machine tools can no longer meet people's needs. People have proposed a mineral casting composed of resin and stone fragments as aggregates. The thermal expansion coefficient of mineral castings is similar to that of steel and can be used in conjunction with metal parts. The shock absorption of mineral castings is much better than that of gray cast iron. The vibration of machine tools using mineral castings has almost no effect during the processing process, which can ensure the accuracy of machine tools and improve the accuracy of processed workpieces. In addition, mineral castings are not sensitive to temperature changes and have much lower thermal conductivity than metals. They effectively control the dimensional error caused by thermal expansion of machine tools to a minimum, ensuring the accuracy of machine tools, and can be used to process high-precision parts.
[0004] The mechanical strength of mineral castings is lower than that of metal castings. They are prone to cracking and breaking when impacted, and the cracks are mainly concentrated at the bonding interface between the resin and the stone, causing the resin bonding interface to be completely peeled off from the stone surface. The applicant has proposed a mineral casting with good resin-mineral aggregate bonding, which can effectively solve the problem of low mechanical strength and easy breakage of mineral castings. Summary of the invention
[0005] The object of the present invention is to provide a high-strength mineral composite casting formula to solve the problems mentioned in the background technology.
[0006] To achieve the above object, the present invention provides the following specific formula, which comprises 60-70 parts of pretreated granite, the pretreatment step comprising soaking the granite in water for 24 hours and then freezing it at sub-zero temperature for 90 minutes, and then flame-uniformly calcining the surface of the granite, the granite particle size is not less than 20 mm, 30-40 parts of bisphenol A novolac epoxy resin prepolymer, 10-20 parts of bisphenol F benzoxazine, 1-2 parts of N-aminoethyl piperazine, 0.1-0.5 parts of titanium tetrachloride, 1-5 parts of corundum powder, 0.05-0.1 of non-floating aluminum powder, 0.2-0.5 parts of stone powder, 1-2 parts of aramid 1414 fiber with a length of not less than 30 mm, and 1-3 parts of sepiolite.
[0007] Furthermore, the granite is a mixture of coarse-grained gray granite, coarse-grained white granite, and coarse-grained yellow granite in any proportion.
[0008] Furthermore, the sepiolite is vacuum ground to 800 mesh.
[0009] In addition, the present invention also provides a production process matching the above-mentioned mineral casting formula, comprising the following steps:
[0010] (a) Crushing granite, wherein 40% of the granite particles are of 1-8 mm in diameter, 30% of the granite particles are of 8-18 mm in diameter, and 30% of the granite particles are of 18-32 mm in diameter. After washing away the powder and debris, the particles are soaked in clean water for 24 hours to fully absorb water;
[0011] (b) The granite is transferred to sub-zero temperature and frozen for 90 minutes, and then the granite surface is evenly calcined with a 2000-2850°C petroleum gas flame;
[0012] (c) mixing bisphenol A novolac epoxy resin prepolymer and titanium tetrachloride, and mixing bisphenol F benzoxazine and N-aminoethylpiperazine;
[0013] (d) Corundum powder, aramid 1414 fiber, non-leafing aluminum powder, and sepiolite are added to bisphenol A novolac epoxy resin prepolymer and bisphenol F benzoxazine in equal parts and mixed.
[0014] (e) heating the bisphenol A novolac epoxy resin prepolymer to 50-60° C. and stirring evenly;
[0015] (f) heating bisphenol F benzoxazine to 80-90° C. and stirring for 10 min;
[0016] (g) bisphenol A novolac epoxy resin and bisphenol F benzoxazine are mixed and stirred uniformly;
[0017] (h) removing debris from the surface of the granite, selecting a mold to evenly place the granite, pouring the mixture from step (g) into the mold, and vibrating in a vacuum environment to remove bubbles;
[0018] (i) Place the mold in a vacuum oven, heat it to 80-90°C and dry it for 30 minutes, then heat it to 120-140°C for 60 minutes.
[0019] (j) Take out the mold and cool it to room temperature.
[0020] Furthermore, the same part of the granite surface should not be calcined continuously for more than 30 seconds. The purpose of this step is to avoid the local temperature being too high and causing the granite to crack.
[0021] Furthermore, the method further comprises step (k) annealing to eliminate internal stress.
[0022] Furthermore, the heating operation is specifically to place the mold into a vacuum oven, heat it to 60°C for 60 minutes, then heat it to 120°C for 180 minutes, and naturally cool it to room temperature.
[0023] N-Aminoethylpiperazine is a colorless or light yellow transparent liquid. Its addition purpose is to promote the cross-linking and curing of bisphenol A novolac epoxy resin prepolymer.
[0024] Titanium tetrachloride is a colorless or slightly yellow liquid at room temperature. Its addition purpose is to promote the cross-linking and curing of bisphenol F-type benzoxazine, and solve the problem of too high curing temperature of bisphenol F-type benzoxazine during heating and curing.
[0025] White Fused Alumian Micropowder, also known as white corundum micropowder, has good chemical stability and high hardness. Its main component is α-Al2O3. It is added as a filler to increase the strength and wear resistance of castings.
[0026] Non-leafing aluminum powder (Silver powder), also known as silver powder and silver paste, is a metallic pigment with good hiding power and is generally used to make coatings. The purpose of adding non-leafing aluminum powder to mineral castings is to give the ore castings conductivity to reduce the accumulation of static electricity on the castings. At the same time, non-leafing aluminum powder as a filler can enhance the strength of the resin after cross-linking and curing, thereby improving the mechanical strength of the casting.
[0027] Aramid 1414 fiber has good high temperature resistance and excellent tensile strength. Its addition purpose is to increase the overall strength of the casting and avoid the problem of casting peeling after fracture.
[0028] The purpose of adding sepiolite is to avoid the non-floating aluminum powder settling which leads to uneven conductivity of the casting as a whole. The structure of sepiolite is loose and porous. After absorbing bisphenol A novolac epoxy resin prepolymer and bisphenol F benzoxazine and then being cross-linked and cured, it can perfectly combine with the two.
[0029] The invention provides a high-strength mineral composite casting formula and a production and preparation process thereof. By preparing a granite aggregate with micro cracks and pores and combining it with an IPN resin with a spatial hinge network structure, a unique intrusive interface can be formed between the resin and the granite aggregate. The bonding strength is high and the interface peeling problem is not likely to occur. The invention has practical significance and promotion value and is expected to generate good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0031] Figure 1 It is a schematic diagram of the surface structure of a high-strength mineral composite casting;
[0032] Figure 2 It is a schematic diagram of the cross-sectional structure of a high-strength mineral composite casting; DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] 60 parts of pretreated granite, 30 parts of bisphenol A novolac epoxy resin prepolymer, 10 parts of bisphenol F benzoxazine, 1 part of N-aminoethyl piperazine, 0.2 parts of titanium tetrachloride, 1 part of corundum powder, 0.08 parts of non-leafing aluminum powder, 0.3 parts of stone powder, 1 part of aramid 1414 fiber with a length not less than 30 mm, and 1 part of sepiolite.
[0036] Example 2
[0037] 60 parts of pretreated granite, 35 parts of bisphenol A novolac epoxy resin prepolymer, 10 parts of bisphenol F benzoxazine, 1 part of N-aminoethyl piperazine, 0.2 parts of titanium tetrachloride, 1 part of corundum powder, 0.08 parts of non-leafing aluminum powder, 0.3 parts of stone powder, 1 part of aramid 1414 fiber with a length not less than 30 mm, and 1 part of sepiolite.
[0038] Example 3
[0039] 60 parts of pretreated granite, 40 parts of bisphenol A novolac epoxy resin prepolymer, 10 parts of bisphenol F benzoxazine, 1 part of N-aminoethyl piperazine, 0.2 parts of titanium tetrachloride, 1 part of corundum powder, 0.08 parts of non-leafing aluminum powder, 0.3 parts of stone powder, 1 part of aramid 1414 fiber with a length not less than 30 mm, and 1 part of sepiolite.
[0040] Example 4
[0041] 60 parts of pretreated granite, 30 parts of bisphenol A novolac epoxy resin prepolymer, 15 parts of bisphenol F benzoxazine, 1 part of N-aminoethyl piperazine, 0.2 parts of titanium tetrachloride, 1 part of corundum powder, 0.08 parts of non-leafing aluminum powder, 0.3 parts of stone powder, 1 part of aramid 1414 fiber with a length not less than 30 mm, and 1 part of sepiolite.
[0042] Example 5
[0043] 60 parts of pretreated granite, 30 parts of bisphenol A novolac epoxy resin prepolymer, 20 parts of bisphenol F benzoxazine, 1 part of N-aminoethyl piperazine, 0.2 parts of titanium tetrachloride, 1 part of corundum powder, 0.08 parts of non-leafing aluminum powder, 0.3 parts of stone powder, 1 part of aramid 1414 fiber with a length not less than 30 mm, and 1 part of sepiolite.
[0044] The above embodiments are all prepared using the same preparation process, and the specific steps are as follows:
[0045] (a) Crushing granite, wherein 40% of the granite particles are of 1-8 mm in diameter, 30% of the granite particles are of 8-18 mm in diameter, and 30% of the granite particles are of 18-32 mm in diameter. After washing away the powder and debris, the particles are soaked in clean water for 24 hours to fully absorb water;
[0046] (b) The granite is transferred to sub-zero temperature and frozen for 90 minutes, and then the granite surface is evenly calcined with a 2000-2850℃ petroleum gas flame. The same part of the granite surface is calcined continuously for at least 20 seconds and should not be calcined continuously for more than 30 seconds to avoid cracking of the granite surface to form a litchi surface;
[0047] (c) mixing bisphenol A novolac epoxy resin prepolymer and titanium tetrachloride, and mixing bisphenol F benzoxazine and N-aminoethylpiperazine;
[0048] (d) Corundum powder, aramid 1414 fiber, non-leafing aluminum powder, and sepiolite are added to bisphenol A novolac epoxy resin prepolymer and bisphenol F benzoxazine in equal parts and mixed.
[0049] (e) heating the bisphenol A novolac epoxy resin prepolymer to 50-60° C. and stirring evenly;
[0050] (f) heating bisphenol F benzoxazine to 80-90° C. and stirring for 10 min;
[0051] (g) bisphenol A novolac epoxy resin and bisphenol F benzoxazine are mixed and stirred uniformly;
[0052] (h) removing debris from the surface of the granite, selecting a mold to evenly place the granite, pouring the mixture from step (g) into the mold, and vibrating in a vacuum environment to remove bubbles;
[0053] (i) Place the mold in a vacuum oven, heat it to 80-90°C and dry it for 30 minutes, then heat it to 120-140°C for 60 minutes.
[0054] (j) taking out the mold and cooling it to room temperature;
[0055] (k) Annealing to eliminate internal stress. The annealing operation is to place the mold in a vacuum oven, heat it to 60°C for 60 minutes, then heat it to 120°C for 180 minutes, and naturally cool it to room temperature.
[0056] Table 1. Comparison of physical properties of high-strength mineral composite castings (Example 3) with gray cast iron and granite
[0057]
[0058] Combined with Table 1, it can be seen that the high-strength mineral composite castings have excellent mechanical properties and have the potential for application as lathe castings.
[0059] Table 2. Comparison of thermal stability between high-strength mineral composite castings and gray cast iron (101 kPa)
[0060]
[0061] Note: Measured by infrared electronic thermometer
[0062] Combined with Table 2, under the same environment, after 96 hours of continuous measurement, by comparing the temperature changes of the two materials, it can be seen that the thermal stability of the mineral composite casting is better than that of gray cast iron.
[0063] After the granite is crushed to the required particle size, it is soaked to absorb sufficient water. In a low-temperature environment, the volume expansion of water when it freezes will form microscopic cracks inside the granite. Subsequently, during the flame calcination process, the flame calcination will also remove low-melting-point impurities such as tourmaline, titanite, plagioclase and amphibole on the surface of the granite particles, which helps to form deep pores on the surface of the granite. The resin component penetrates into the cracks and pores of the granite particles to form an invasive interface with high bonding strength, making it less likely for interface peeling to occur.
[0064] Bisphenol A novolac epoxy resin prepolymer is cross-linked and cured under the catalysis of N-aminoethylpiperazine to form a spatial network structure, and bisphenol F benzoxazine is cross-linked and cured under the catalysis of titanium tetrachloride to form a spatial network structure. Since the bisphenol A novolac epoxy resin prepolymer and bisphenol F benzoxazine are mixed and the two components have good compatibility, an IPN (Interpenetrating Polymer Network) network will be formed, which helps to improve the strength of the resin component and avoid the problem of brittle fracture.
[0065] It will be easily understood by those skilled in the art that the above description is merely an example of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high-strength mineral composite casting formula, characterized in that: By weight, including: 60-70 parts of pre-treated granite, the pre-treatment steps include soaking the granite in water for 24 hours, freezing it at sub-zero temperature for 90 minutes, and then flame calcining the granite surface evenly, and the granite particle size is not less than 20mm; 30-40 parts of bisphenol A novolac epoxy resin prepolymer; 10-20 parts of bisphenol F type benzoxazine; 1-2 parts of N-aminoethylpiperazine; 0.1-0.5 parts of titanium tetrachloride; 1-5 parts of corundum powder; Non-leafing aluminum powder 0.05-0.1 part; Stone powder 0.2-0.5 parts; 1-2 parts of aramid 1414 fiber, length not less than 30mm; 1-3 parts of sepiolite.
2. A high-strength mineral composite casting formula according to claim 1, characterized in that: The granite is a mixture of coarse-grained gray granite, coarse-grained white granite and coarse-grained yellow granite in any proportion.
3. A high-strength mineral composite casting formula according to claim 1, characterized in that: Sepiolite was vacuum ground to 800 mesh.
4. A production process for preparing the high-strength mineral composite casting formula according to any one of claims 1 to 3, characterized in that: The steps include: (a) Crushing granite, wherein 40% of the granite particles are of 1-8 mm in diameter, 30% of the granite particles are of 8-18 mm in diameter, and 30% of the granite particles are of 18-32 mm in diameter. After washing away the powder and debris, the particles are soaked in clean water for 24 hours to fully absorb water; (b) The granite is transferred to sub-zero temperature and frozen for 90 minutes, and then the granite surface is evenly calcined with a 2000-2850°C petroleum gas flame; (c) mixing bisphenol A novolac epoxy resin prepolymer and titanium tetrachloride, and mixing bisphenol F benzoxazine and N-aminoethylpiperazine; (d) Corundum powder, aramid 1414 fiber, non-leafing aluminum powder, and sepiolite are added to bisphenol A novolac epoxy resin prepolymer and bisphenol F benzoxazine in equal parts and mixed. (e) heating the bisphenol A novolac epoxy resin prepolymer to 50-60° C. and stirring evenly; (f) heating bisphenol F benzoxazine to 80-90° C. and stirring for 10 min; (g) bisphenol A novolac epoxy resin and bisphenol F benzoxazine are mixed and stirred uniformly; (h) removing debris from the surface of the granite, selecting a mold to evenly place the granite, pouring the mixture from step (g) into the mold, and vibrating in a vacuum environment to remove bubbles; (i) Place the mold in a vacuum oven, heat it to 80-90°C and dry it for 30 minutes, then heat it to 120-140°C for 60 minutes. (j) Take out the mold and cool it to room temperature.
5. The production process of a high-strength mineral composite casting according to claim 4, characterized in that: The same part of the granite surface shall not be calcined continuously for more than 30 seconds.
6. A production process for a high-strength mineral composite casting according to any one of claims 4 and 5, characterized in that: The method further comprises the step (k) of annealing to eliminate internal stress.
7. The production process of a high-strength mineral composite casting according to claim 6, characterized in that: The annealing operation is specifically to place the mold in a vacuum oven, heat it to 60°C for 60 minutes, then heat it to 120°C for 180 minutes, and naturally cool it to room temperature.