Method for preparing cementing material for mine filling by using suspension roasting iron separation tailings
By combining suspension roasting iron tailings with composite powder and chemical activators, a cementitious material for mine backfilling was prepared, solving the problem of resource utilization of suspension roasting iron tailings and realizing low-cost, environmentally friendly cementitious material production and high-performance backfill preparation.
Patent Information
- Application Number
- CN202410977050.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-22
Smart Images

Figure BDA0004954893090000051 
Figure BDA0004954893090000052 
Figure BDA0004954893090000053
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of cementitious materials for tailings filling, and in particular relates to a method for preparing a mine filling cementitious material by utilizing suspended roasting of iron ore tailings. Background Art
[0002] At present, most of the cementitious materials used in mines are made of cement clinker, slag, gypsum and other activators, and the cost is relatively high. For example, the Chinese patent (CN201510166877) uses blast furnace water-quenched slag, fly ash, cement clinker, lime and gypsum in proportion to prepare a new type of cementing agent for tailings consolidation and discharge. Although the strength of the filling body can meet the requirements, the raw material cost of this method is relatively high. For ordinary tailings-based cementitious materials, since the activity of the tailings themselves is very low, high-temperature thermal activation or chemical agent treatment is usually required to make cementitious materials, resulting in high costs and difficulty in industrialization. For example, a tailings-based cementitious material and its preparation method disclosed in the Chinese patent (CN2020107722659) is to dry the tailings and then perform mechanical ball milling activation treatment, thermal activation treatment and chemical agent activation treatment in sequence to obtain a tailings-based cementitious material. Although the performance of the cementitious material obtained by this method can meet the requirements of the downhole filling process, its thermal activation process requires a high temperature of 300 to 1000°C, so it not only consumes a lot of energy, but also causes great pollution.
[0003] Most of the iron ore in my country is difficult to select, and the suspension roasting magnetic separation technology is a new technology for processing difficult-to-select iron ore. Compared with traditional strong magnetic and flotation technologies, the suspension roasting magnetic separation technology can greatly improve the concentrate grade and metal recovery rate, so it has a very broad application prospect. This technology has been industrialized in Jiugang Ore Dressing Plant and has achieved good technical and economic indicators. At present, the suspension roasting magnetic separation production line of Hainan Iron Mine has also been built and production commissioning is underway. With the large-scale promotion and application of suspension roasting magnetic separation technology in the future, a large amount of suspension roasting magnetic separation iron tailings will inevitably be generated. If these tailings cannot be reasonably utilized, they will not only occupy a large amount of storage land, but also have a serious impact on the ecological environment. Because the industrial application time of suspension roasting magnetic separation technology is not long, there is little research on the resource utilization of suspension roasting iron tailings, and there are basically no relevant technical patents disclosed.
[0004] Since the suspended roasted iron tailings are not only fine in particle size (usually below 74 microns) but also roasted at high temperature, they usually have a certain activity and have the potential to be used as a raw material for cementitious materials for mine filling. Based on the above considerations, the present invention prepares a new type of cementitious material for mine filling by mechanically grinding and chemically activating the suspended roasted iron tailings, which not only realizes the resource utilization of the suspended roasted iron tailings, but also reduces the production cost of the cementitious material. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a cementitious material for mine filling by using suspended roasting iron tailings to address the technical problems of large amount of iron tailings produced, difficult disposal and difficult resource utilization in the existing suspended roasting iron tailings.
[0006] To achieve the above-mentioned purpose of the present invention, the method for preparing a cementitious material for mine filling by suspended roasting of iron ore tailings adopts the following technical scheme.
[0007] The cementitious material for mine filling is prepared by mixing the following components, and the mass proportion of each component when the sum of the raw material components is 100% is: 24% to 35% of suspended roasting iron ore tailings, 63.5% to 74.7% of composite powder, and 0.3% to 1.5% of activator; the composite powder is prepared by mixing slag powder, desulfurized gypsum, and cement in proportion; the activator is prepared by mixing sodium ethyl silicate, sodium sulfate, sodium lignin sulfonate, and triethanolamine in proportion.
[0008] Furthermore, the suspension roasting iron tailings are crushed and ground to a fineness of -38 microns accounting for more than 90%. Generally, the suspension roasting iron tailings are naturally dried and then crushed to -2mm in two stages using a jaw crusher and a roller crusher, and then the crushed products are dry-ground using a ball mill to a fineness of -38 microns accounting for more than 90%.
[0009] Furthermore, when the sum of the components in the composite powder is 100%, the mass proportion of each component is: 40% to 60% of slag powder, 20% to 30% of desulfurized gypsum, and 20% to 30% of cement.
[0010] Furthermore, the slag powder is of S105 grade, with a specific surface area of ≥700m 2 / kg; the desulfurized gypsum is an industrial product, with a β-hemihydrate gypsum content of >70%, a 0.2mm square hole sieve residue of <5%, an initial setting time of >5min, a final setting time of <25min, and a 2h compressive strength of ≥6MPa; the cement is 42.5 # Ordinary Portland cement.
[0011] Furthermore, the mass proportion of each component in the stimulator when the sum of the components is 100% is: 30% to 35% of ethyl sodium silicate, 30% to 35% of sodium sulfate, 30% to 35% of sodium lignin sulfonate, and 3% to 10% of triethanolamine; the sodium ethyl silicate, sodium sulfate, sodium lignin sulfonate, and triethanolamine are mixed in proportion and dry-ground in a ball mill to a fineness of -38 microns accounting for more than 90%; the sodium ethyl silicate, sodium sulfate, sodium lignin sulfonate, and triethanolamine are all industrial products, and the content of effective ingredients is greater than 90%.
[0012] The principle of using high-temperature roasted iron tailings as raw materials for preparing cementitious materials for mine filling in the present invention is that after the difficult-to-select iron ore is subjected to high-temperature suspension roasting treatment, the high-temperature roasted iron tailings discharged after the iron ore is recovered through grinding-magnetic separation have similar characteristics to volcanic ash, and contain relatively high active components such as active silicon dioxide and active alumina. These active components are easy to react with calcium hydroxide in the filling tailings to generate reaction products such as hydrated calcium silicate, hydrated calcium aluminate or hydrated calcium sulfoaluminate, thereby greatly improving the strength of the filling body. Therefore, high-temperature roasted iron tailings can be used as raw materials for preparing cementitious materials for mine filling.
[0013] Compared with the prior art, the method of preparing a cementitious material for mine filling by suspended roasting of iron ore tailings has the following beneficial effects:
[0014] (1) The use of suspended roasted iron tailings as the raw material of cementitious materials for mine filling is the first time that mine tailings are used as the raw material of cementitious materials for mine filling. It not only expands the raw material source of cementitious materials, but also greatly reduces the production cost of cementitious materials. At the same time, it realizes the resource utilization of suspended roasted iron tailings and reduces the land occupied by suspended roasted iron tailings and the harm to the environment.
[0015] (2) The slag powder and desulfurized gypsum, which are the main raw materials of the cementitious material prepared by the method of the present invention, are both industrial by-products with wide sources and low prices.
[0016] (3) The method of the present invention uses mechanical grinding and a combination of chemical stimulants for activation, which further stimulates the activity of the suspended roasting iron ore tailings, so that the prepared cementitious material can be used as a binder for fine-grained tailings, and the performance of the cementitious body meets the requirements of normal filling.
[0017] (4) The production process of the cementitious material prepared by the method of the present invention does not require high temperature, and only has grinding and mixing steps. The production process is simple, environmentally friendly, and requires little investment.
[0018] (5) Compared with the binders for cementing fine-grained tailings filling sold on the market, the production cost (including raw material cost) is reduced by more than 30%. DETAILED DESCRIPTION
[0019] To describe the present invention, the method for preparing a cementitious material for mine filling by suspended roasting of iron ore tailings is further described in detail below in conjunction with the examples. However, the present invention is not limited to the examples.
[0020] The suspension roasting iron-selected tailings used in the method of the present invention are tailings discharged after suspension roasting of a domestic specular iron ore. The specular iron ore is a difficult-to-select iron ore and cannot be separated and enriched by conventional physical beneficiation methods. It needs to be treated by magnetic roasting (suspension roasting) before it can be sorted. In the embodiment, the method of preparing a cementitious material for mine filling using suspension roasting iron-selected tailings of the present invention is specifically implemented as follows:
[0021] (1) After the suspended roasted iron tailings are naturally dried, they are crushed to -2 mm in two stages using a jaw crusher and a roller crusher, and then the crushed products are dry-ground using a ball mill to a fineness of -38 microns accounting for more than 90%, and then used for standby;
[0022] (2) Mix slag powder, desulfurized gypsum and cement according to the proportions in Table 1 to obtain three composite powders with different proportions for standby use. The slag powder is S105 grade with a specific surface area of ≥700m 2 / kg; the desulfurized gypsum is an industrial product, with a β-hemihydrate gypsum content of >70%, a 0.2mm square hole sieve residue of <5%, an initial setting time of >5min, a final setting time of <25min, and a 2h compressive strength of ≥6MPa; the cement is 42.5 # Ordinary Portland cement;
[0023] (3) Sodium ethyl silicate, sodium sulfate, sodium lignin sulfonate and triethanolamine are mixed in the proportions described in Table 2, and then dry-ground by a ball mill to a fineness of -38 microns accounting for more than 90%, to obtain three activators with different proportions for standby use. The sodium ethyl silicate, sodium sulfate, sodium lignin sulfonate and triethanolamine are all industrial products, and the content of effective ingredients is greater than 90%.
[0024] (4) The suspended roasted iron tailings, composite powder and activator obtained in steps (1), (2) and (3) are mixed in the proportions described in Table 3 to obtain three different proportions of cementitious materials for mine filling.
[0025] Table 1 Composite powder formula used in the method of the present invention (mass percentage)
[0026]
[0027] Table 2 Exciter formulation used in the method of the present invention (mass percentage)
[0028]
[0029] Table 3 Formula of cementitious material for mine filling prepared by the method of the present invention (mass percentage)
[0030]
[0031] In the embodiment, the cementing material for mine filling prepared by the method of the present invention is used to perform cementing tests on two fine iron tailings taken from different mines in China, one of which is magnetite tailings, and its particle size composition results are shown in Table 4, and the content of -0.076mm in the tailings is 90.61%; the other is hematite tailings, and its particle size composition results are shown in Table 5, and the content of -0.076mm in the tailings is 95.50%. Both tailings in the embodiment are fine particles that are difficult to cement and fill.
[0032] Table 4 Analysis of particle size composition of a magnetite tailings (%)
[0033]
[0034]
[0035] Table 5 Analysis of particle size composition of a hematite tailings (%)
[0036]
[0037] The three proportions of cementitious materials prepared by the method of the present invention and the comparative example - the invention patent product "a binder for cementing fine tailings" (patent number: ZL201610106411.8) were mixed with the hematite or magnetite tailings described in step 1 at a ratio of 1:6, and then water was added to form a filling slurry with a solid mass concentration of 60%. The slurry was cast into a 70.7mm×70.7mm×70.7mm triple test block, which was placed in a standard cement curing box and cured at a constant temperature (20℃) and constant humidity (90%). After one day, the mold was removed and the curing continued to the specified age. The compressive strength of the cemented filling body at different curing ages was tested by an automatic press. The test results are shown in Tables 6 and 7. Experiments show that, by using three cementitious materials with different proportions prepared by the method of the present invention to cement two types of iron tailings, the filling performance requirements of strength greater than 0.5MP in 3 days, strength greater than 1.0MP in 7 days, and strength greater than 2.5MP in 28 days can be achieved, and the compressive strength at the same time is better than that of the comparative patented product "a binder for cementing and filling of fine-grained tailings", while the cost is less than 70% of that of the comparative example, achieving unexpected technical effects.
[0038] Table 6 Strength of cemented filling body of a fine-grained magnetite tailings (MPa)
[0039]
[0040] Table 7 Strength of cemented filling body of a fine-grained hematite tailings (MPa)
[0041]
Claims
1. A method for preparing a cementitious material for mine filling by suspended roasting of iron ore tailings, characterized in that: The cementitious material for mine filling is prepared by mixing the following components, and the mass proportion of each component when the sum of the raw material components is 100% is: Suspended roasting of iron tailings 24% to 35%; Composite powder 63.5%~74.7%; Exciter 0.3%~1.5%; The composite powder is prepared by mixing slag powder, desulfurized gypsum and cement in a certain proportion; the activator is prepared by mixing sodium ethyl silicate, sodium sulfate, sodium lignin sulfonate and triethanolamine in a certain proportion.
2. The method for preparing a cementitious material for mine filling by suspended roasting of iron ore tailings as claimed in claim 1, characterized in that: The suspended roasting iron ore tailings are crushed and ground to a fineness of -38 microns, which accounts for more than 90% of the powder.
3. The method for preparing a cementitious material for mine filling by suspended roasting of iron ore tailings as claimed in claim 1, characterized in that The mass proportion of each component in the composite powder when the sum of the components is 100% is: Slag powder 40% to 60%; Desulfurized gypsum 20%~30%; Cement 20%~30%.
4. The method for preparing a cementitious material for mine filling by suspended roasting of iron ore tailings as claimed in claim 3, characterized in that: The slag powder is of grade S105, with a specific surface area of ≥700m 2 / kg; the desulfurized gypsum is an industrial product, with a β-hemihydrate gypsum content of >70%, a 0.2mm square hole sieve residue of <5%, an initial setting time of >5min, a final setting time of <25min, and a 2h compressive strength of ≥6MPa; the cement is 42.5 # Ordinary Portland cement.
5. The method for preparing a cementitious material for mine filling by suspended roasting of iron ore tailings as claimed in claim 1, characterized in that The mass proportion of each component in the exciter when the sum of the components is 100% is: Sodium ethyl silicate 30% to 35%; Sodium sulfate 30%-35%; Sodium lignin sulfonate 30% to 35%; Triethanolamine 3%~10%.
6. The method for preparing a cementitious material for mine filling by suspended roasting of iron ore tailings as claimed in claim 5, characterized in that: The sodium ethyl silicate, sodium sulfate, sodium lignin sulfonate and triethanolamine are mixed in proportion and dry-ground in a ball mill to a fineness of -38 microns accounting for more than 90%.
7. The method for preparing a cementitious material for mine filling by suspended roasting of iron ore tailings as claimed in claim 2, characterized in that: The mass proportion of each component in the composite powder when the sum of the components is 100% is: slag powder 40% to 60%, desulfurized gypsum 20% to 30%, cement 20% to 30%; The slag powder is of grade S105, with a specific surface area of ≥700m 2 / kg; the desulfurized gypsum is an industrial product, with a β-hemihydrate gypsum content of >70%, a 0.2mm square hole sieve residue of <5%, an initial setting time of >5min, a final setting time of <25min, and a 2h compressive strength of ≥6MPa; the cement is 42.5 # Ordinary Portland cement; The mass proportion of each component in the stimulator when the sum of the components is 100% is: 30% to 35% of ethyl sodium silicate, 30% to 35% of sodium sulfate, 30% to 35% of sodium lignin sulfonate, and 3% to 10% of triethanolamine; the sodium ethyl silicate, sodium sulfate, sodium lignin sulfonate, and triethanolamine are mixed in proportion and dry-ground in a ball mill to a fineness of more than -38 microns and accounting for more than 90%; sodium ethyl silicate, sodium sulfate, sodium lignin sulfonate, and triethanolamine are all industrial products, and the content of effective ingredients is greater than 90%.
Citation Information
Patent Citations
Building hollow brick using industrial tailings and preparation method thereof
CN102503263A
Preparation process for preparing recycled aggregate based on tailings and aggregate
CN112777957A
Road based on coal gangue and construction method thereof
CN116254735A
Calcined clay tailings and / or calcined mine waste, and associated systems and methods
US20220195306A1
A concrete admixture using waste tailing and methode of thereof
WO2006126752A1