Lightweight high-strength geopolymer-based composite material and preparation method thereof

By using lightweight, high-strength earth polymer-based composite materials in building materials, the application limitations of traditional concrete in high-rise buildings and large-span bridge projects are solved, and material density reduction, strength improvement and toughness enhancement are achieved, and environmental pollution is reduced.

CN118930141AInactive Publication Date: 2024-11-12GUANGDONG UNIV OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410986790.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional concrete has major problems such as low strength, poor toughness, insufficient durability and serious environmental pollution, which limits its application in high-rise buildings and large-span bridges.

Method used

Using lightweight, high-strength earth polymer-based composite material, consisting of hollow glass microbeads, PE fibers, slag, fly ash, alkali trigger and water. Through specific mixing ratios and preparation methods, the formation density is low, the process is simple and has Material with excellent comprehensive performance.

Benefits of technology

It has achieved the reduction of density, strength and toughness of materials, and is suitable for the field of building materials, with good application prospects and reduced environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930141A_ABST
    Figure CN118930141A_ABST
Patent Text Reader

Abstract

The invention discloses a lightweight high-strength geopolymer-based composite material and a preparation method thereof, and relates to the technical field of building materials. The lightweight high-strength geopolymer-based composite material is prepared by doping the hollow glass beads (HGM) and the PE fibers into the cementing material prepared from the fly ash and the slag, and the lightweight high-strength geopolymer-based composite material is low in density, simple in preparation process and excellent in comprehensive performance, and shows a good application prospect in the field of building materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a lightweight and high-strength geopolymer-based composite material and a preparation method thereof. Background Art

[0002] With the continuous development of the construction industry, a large number of high-rise buildings, long-span bridges and marine projects have emerged, and people's demand for high-performance concrete has become increasingly strong. However, traditional ordinary concrete has problems such as heavy weight, low strength (especially flexural strength), poor toughness, insufficient durability, high consumption of natural resources and serious environmental pollution, which restrict its application.

[0003] Based on the above development background, lightweight, high ductility, high strength green concrete materials have become a hot research direction. Therefore, it is extremely necessary to provide a new type of lightweight and high strength geopolymer-based composite material with excellent performance. Summary of the invention

[0004] The purpose of the present invention is to provide a lightweight and high-strength geopolymer-based composite material and a preparation method thereof, so as to solve the problems existing in the above-mentioned prior art.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] The present invention provides a lightweight and high-strength geopolymer-based composite material, the raw materials of which are composed of the following components:

[0007] Hollow glass microspheres, PE fibers, slag, fly ash, alkali activator, retarder and water; the volume proportion of the hollow glass microspheres in the raw materials is 8.6%-36.8%; the volume proportion of the PE fibers in the raw materials is 2%.

[0008] Furthermore, the density of the hollow glass microspheres is 0.2-0.6 g / cm 3 , the compressive strength is 10-55MPa.

[0009] Furthermore, the particle size of the hollow glass microspheres is 45-60 μm.

[0010] Furthermore, the alkaline activator is prepared by mixing a 2.25 modulus sodium silicate solution and a 10 mol / L sodium hydroxide solution in a mass ratio of 2:1.

[0011] Furthermore, the raw material ratio is as follows:

[0012] Fly ash 406-586.8kg / m 3 , slag 406-586.8kg / m 3 , hollow glass microspheres 35.4-147.3kg / m 3, sodium hydroxide solution 108.4-149.8kg / m 3 , sodium silicate solution 216.9-312.9kg / m 3 , water 48.7-70.3kg / m 3 , retarder 8.1-11.7kg / m 3 , PE fiber 19.4kg / m 3 .

[0013] The present invention also provides a method for preparing the above-mentioned light-weight high-strength geopolymer-based composite material, which comprises uniformly mixing raw materials to prepare the light-weight high-strength geopolymer-based composite material.

[0014] The present invention discloses the following technical effects:

[0015] The present invention mixes hollow glass microspheres (HGM) and PE fibers into a cementitious material prepared from fly ash and slag to prepare a lightweight high-strength geopolymer-based composite material. The lightweight high-strength geopolymer-based composite material has low density, simple preparation process, excellent comprehensive performance, and shows good application prospects in the field of building materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 (a) shows the effect of aggregate type on the pseudo strain hardening index and density of LWHS-EGC, and (b) shows the effect of HGM40 volume ratio on the pseudo strain hardening index of LWHS-EGC (the density of the single crack axial tension test corresponds to the ordinate value on the left, PSH S The indicator corresponds to the first vertical axis on the right, PSH E The indicator corresponds to the second vertical axis on the right).

[0017] Figure 2 (a) shows the effect of aggregate type on mortar fluidity, and (b) shows the effect of HGM40 volume proportion on mortar fluidity.

[0018] Figure 3 Failure mode of LWHS-EGC cylindrical specimen.

[0019] Figure 4 is the static axial compressive stress-strain curve of LWHS-EGC; among them, (a), (b), (c), (d), (e), (f), (g), (h), (i), (j), and (k) are the tensile-strain curves of groups 0-4, 6-4, 2-4, 4-2, 4-3, 4-4, 4-5, 4-6, 4-8, 4-10, and 4-12, respectively.

[0020] Figure 5 The effect of aggregate type on static axial compression performance.

[0021] Figure 6 The influence of HGM40 volume ratio on the static axial compression performance.

[0022] Figure 7 (a) is the failure mode of the axial tension specimen after loading; (b) is the effect of different aggregate types on the static axial tension failure mode of LWHS-EGC; (c) is the effect of different volume proportions of HGM40 on the static axial tension failure mode of LWHS-EGC.

[0023] Figure 8 is the static axial tensile stress-strain curve of LWHS-EGC; among them, (a), (b), (c), (d), (e), (f), (g), (h), (i), (j), and (k) are the tensile-strain curves of groups 0-4, 6-4, 2-4, 4-2, 4-3, 4-4, 4-5, 4-6, 4-8, 4-10, and 4-12, respectively.

[0024] Fig. 9 The effect of different aggregate types on the static axial tension properties of LWHS-EGC.

[0025] Fig.10 The effect of different volume proportions of HGM40 on the static axial tensile properties of LWHS-EGC.

[0026] Fig.11 are the stress-strain curves of the dynamic compression test of LWHS-EGC; (a), (b), (c), (d), (e), (f), (g), (h), (i), (j), and (k) are the tensile-strain curves of groups 0-4, 6-4, 2-4, 4-2, 4-3, 4-4, 4-5, 4-6, 4-8, 4-10, and 4-12, respectively.

[0027] Fig.12 The influence of aggregate type on the dynamic compression properties of LWHS-EGC; (a) is the peak stress at different strain rates, (b) is the impact toughness at different strain rates, and (c) is the DIF at different strain rates.

[0028] Fig.13 The influence of HGM40 volume ratio on the dynamic compression properties of LWHS-EGC; (a) is the peak stress at different strain rates, (b) is the impact toughness at different strain rates, and (c) is the DIF at different strain rates. DETAILED DESCRIPTION

[0029] Various exemplary embodiments of the present invention will now be described in detail, but this detailed description should not be construed as limiting the present invention.

[0030] Example 1

[0031] 1. Experimental materials:

[0032] Slag (GGBS), fly ash (FA), quartz sand, hollow glass microspheres (HGM), alkali activators (NaOH, Na 2 SiO 3 ), ultra-high molecular weight polyethylene fiber (UHMWPE fiber, referred to as PE fiber), retarder (BaCl 2 ) and water. The specific indicators of the raw materials are as follows:

[0033] (1) Fly ash (FA): Class F fly ash, sourced from Gongyi Longze Water Purification Material Co., Ltd., is a black solid powder. The chemical composition and physical parameters are shown in Tables 1 and 2.

[0034] Table 1 Chemical composition of fly ash (unit: %)

[0035]

[0036] Table 2 Physical parameters of fly ash

[0037]

[0038] (2) Slag (GGBS): Blast furnace S105 slag, sourced from Gongyi Longze Water Purification Material Co., Ltd., is a white solid powder. The chemical composition and physical parameters are shown in Table 3-4.

[0039] Table 3 Chemical composition of S105 slag (unit: %)

[0040]

[0041] Table 4 Slag physical parameters

[0042]

[0043] (3) Hollow glass microspheres (HGM): Its composition is 98% to 100% soda lime borosilicate glass and 0% to 2% synthetic amorphous free silica. The structure is a smooth, closed hollow thin-walled sphere with a particle size of 10 to 200 μm and a density of 0.1 to 0.6 g / cm 3 , has certain pozzolanic activity, but its contribution is negligible when added with silica fume and low w / c ratio. 3 , 0.40g / cm 3 and 0.20g / cm 3 There are three different types of hollow microspheres, named HGM60, HGM40 and HGM20. The chemical composition and physical parameters of hollow glass microspheres are shown in Table 5-7.

[0044] Table 5 Chemical composition of hollow glass microspheres (unit: %)

[0045]

[0046] Table 6 Physical parameters of hollow glass microspheres

[0047]

[0048] Table 7 Model parameter table of hollow glass microspheres

[0049]

[0050] (4) Quartz sand: No. 9 quartz sand, specific gravity is 2.65, average diameter is 110 μm.

[0051] (5) Alkali activator: The alkaline activator is prepared by mixing 2.25 modulus sodium silicate solution and 10 mol / L sodium hydroxide solution in a ratio of 2:1. The parameters of the sodium silicate solution are shown in Table 8.

[0052] Table 8 Parameters of sodium silicate solution

[0053]

[0054] (6) PE fiber, sourced from Dongguan Sovit Special Wire Co., Ltd., is white bundled fiber monofilament. The physical properties of PE fiber are shown in Table 9.

[0055] Table 9 PE fiber parameters

[0056]

[0057] (7) Retarder: barium chloride is a white solid that is easily soluble in water. Its dosage is 0.5% to 1% of the amount of cementitious material used.

[0058] (8) The water used is tap water for laboratory use and meets the requirements of relevant national standards.

[0059] 2. Material mix design

[0060] The present invention takes lightweight high-strength geopolymer-based composites (LWHS-EGC) as the research object and designs two research variables. One is different types of aggregates, using three types of hollow glass microspheres of HGM60, HGM40 and HGM20, and a quartz sand group as the control group; the other is the different volume proportions of HGM40, ranging from 8.6% to 36.8%.

[0061] The present invention measures the pseudo strain hardening index of LWHS-EGC to detect whether the conditions for realizing the development of ECC multiple cracks are met, and whether the state of multiple saturated cracks can be further realized. All the mix proportion groups of the present invention are shown in Table 10-Table 11:

[0062] Table 10 LWHS-EGC mix ratios of HGM40 at different volume ratios

[0063]

[0064] Note: The fiber content is 2% by volume; the aggregate volume proportions of groups 4-2, 4-3, 4-4, 4-5, 4-6, 4-8, 4-10 and 4-12 are 8.6%, 12.3%, 15.8%, 19%, 22.6%, 28%, 32.7% and 36.8% respectively, and the type of aggregate is constant as HGM40.

[0065] Table 11 LWHS-EGC mix proportions of different aggregate types

[0066]

[0067] Note: The fiber content is 2% by volume; the aggregate type of group 0-4 is quartz sand, and the aggregate types of groups 6-4, 4-4 and 2-4 are HGM60, HGM40 and HGM20 respectively, and the volume proportion of aggregate is constant at 15.8%.

[0068] In order to make the material have a good ECC effect, from the perspective of the strength criterion, energy criterion and two pseudo strain hardening (PSH) indicators guiding the ECC design, a three-point bending test and a single crack axial tension test of the base beam were carried out to detect whether it has the conditions to realize the development of ECC multiple cracks and whether it can further realize the state of multiple saturated cracks, providing theoretical and data support for subsequent analysis. The design of the mix ratio group is also determined by referring to the results of the matrix fracture test and the single crack axial tension test.

[0069] The fracture toughness of the matrix was first determined by a three-point bending test of the matrix beam. The test was carried out in accordance with the requirements of Fracture Mechanics of Concrete (RILEM FMC-50).

[0070] The fracture toughness of the matrix is ​​calculated according to the following formula:

[0071]

[0072] a=a 0 / h (1.3)

[0073] Among them, F Q is the maximum load value recorded in the three-point bending test of the notched beam, m is the weight of the specimen, g is the acceleration of gravity, which is 9.8 m / s 2 , S is the span of the cut beam, a 0is the seam height, t and h are the width and height of the specimen respectively. f(a) is the shape factor of the beam, which is only related to the size of the beam.

[0074] Table 12 Three-point bending test results of base beam

[0075]

[0076]

[0077] The strength criterion, energy criterion and two pseudo strain hardening (PSH) indices are then determined through single crack axial tension tests.

[0078] ECC is designed based on micromechanics and fracture mechanics, with ultra-high ductility and excellent crack control ability. Its axial tensile limit strain can stably reach more than 3%. There are two criteria that need to be met in the design of ECC, namely the strength (FCS) criterion and the energy (SSC) criterion, also known as the initial crack criterion and the steady-state cracking criterion. Otherwise, it will only have a single crack like ordinary fiber concrete, and once it appears, it will be the peak tensile stress.

[0079] The first crack (FCS) criterion and the steady-state crack (SCC) criterion are shown in equations (2.1)-(2.2) respectively:

[0080] σ ss <σ 0 (2.1)

[0081]

[0082] Among them, σ ss is the matrix cracking strength, σ 0 is the fiber bridging stress, δ 0 corresponds to σ 0 The crack opening displacement, J tip is the crack tip toughness, J b ′ is the fiber bridging residual energy.

[0083] Formula (2.1) indicates that the cracking strength of the matrix must not exceed the maximum fiber bridging stress. This criterion ensures that subsequent cracks can develop before the peak fiber bridging stress is reached, thus achieving the phenomenon of multi-crack cracking.

[0084] Formula (2.2) shows that the crack tip toughness of the matrix should not exceed the complementary energy, which can be calculated from the fiber bridging stress-crack opening displacement (σ-δ) curve. Meeting this criterion can ensure steady-state cracking, that is, when the crack tip expands, the crack width remains basically unchanged.

[0085] Although achieving the above two criteria can achieve multi-crack cracking, which can be called ECC, it is still not enough to form saturated cracks. In order to achieve saturated cracks in ECC materials, Kanda et al. proposed two pseudo strain hardening (PSH) indicators. For ECC using ultra-high molecular weight polyethylene fibers (PE fibers), the two PSH indicators are shown in equations (2.3)-(2.4):

[0086]

[0087]

[0088] The crack tip toughness of the matrix is ​​generally calculated by formula (2.5), but when the fiber volume content is less than 3%, the crack tip toughness of the matrix can be calculated by formula (2.6):

[0089]

[0090] Among them, K m 、E m are the fracture toughness and elastic modulus of the matrix, respectively.

[0091] The determination of the parameters of the two pseudo strain hardening (PSH) indicators needs to be completed through the three-point bending test and uniaxial tensile test of the base beam. The single crack axial tensile test is carried out in accordance with the requirements of the specification "Test Method for Mechanical Properties of High Ductility Fiber Reinforced Cement-based Composite Materials" (JC / T2461-2018).

[0092] Tables 13 and 14 list the fracture toughness J at the crack tip respectively. tip and fiber bridging residual energy J b′ According to the data of the three-point bending test and the single-crack axial tension test of the base beam and their calculation results, Table 15 presents the two pseudo strain hardening (PSH) indicators finally calculated.

[0093] Table 13 Single crack axial tension test results

[0094]

[0095] Table 14 Fracture toughness J at crack tip tip Calculation results

[0096]

[0097] Table 15 Summary of PSH indicators

[0098]

[0099] Figure 1(a) shows the effect of aggregate type on the pseudo strain hardening index and density of LWHS-EGC, and (b) shows the effect of HGM40 volume ratio on the pseudo strain hardening index of LWHS-EGC (the density of the single crack axial tension test corresponds to the ordinate value on the left, PSH S The indicator corresponds to the first vertical axis on the right, PSH E The indicator corresponds to the second vertical axis on the right).

[0100] The 11 mix proportions designed by the present invention not only meet the two ECC design criteria, but also meet the two pseudo strain hardening indicators of ECC, that is, they all meet the PSH E >3 and PSH S >1.2, therefore, the 11 mix proportions designed in the present invention not only have the conditions for realizing the development of ECC multiple cracks, but also have the potential to further realize the state of multiple saturated cracks.

[0101] Furthermore, except for the control group, the density of other groups was lower than 1920 kg / m 3 , meeting the standards for structural lightweight aggregate concrete (LWAC), and several groups have densities below 1500kg / m 3 , meeting the standards of ultra-lightweight cementitious composite materials (ULCC).

[0102] PSH E The index ranges from 78 to 358, meeting the minimum requirement of 3, and is several dozen times higher than the minimum requirement. E The indicators have been significantly improved, from 199 to 358 and 323, respectively, an increase of 80% and 63%; with the increase of HGM volume proportion, PSH E The index first increased and then decreased. In the process of HGM volume proportion increasing from 8.6% to 19%, PSH E The index increased from 274 to 351, an increase of 26%. In the process of HGM volume ratio increasing from 19% to 36.8%, PSH E The index dropped from 351 to 78, a decrease of 78%. PSH S The index ranges from 1.76 to 3.21, meeting the minimum requirement of 1.2, but not exceeding it by much. S The indicators were significantly reduced, from 3.21 to 2.1 and 1.98, respectively, a decrease of 35% and 38%; with the increase of HGM volume proportion, PSH S The index first increased and then decreased. In the process of HGM volume proportion increasing from 8.6% to 19%, PSH SThe index increased from 1.63 to 2.42, an increase of 44%. In the process of HGM volume increasing from 19% to 36.8%, PSH S The indicator decreased by 35% from 2.42 to 1.56.

[0103] 3. Mixing and curing

[0104] Compared with ordinary concrete, the preparation process of fiber composite materials is more difficult and complicated. According to the survey results, the fibers can be evenly dispersed in the matrix to fully exert the toughening effect when the specimen is subjected to external loads. The fibers can bridge cracks and thus play a role in crack resistance. In addition, considering that the coagulation time of geopolymers is short during the preparation process, which will produce a rapid hardening phenomenon, the present invention simultaneously disperses and adds fibers during the mixing process. The specific pouring process is: according to the experimental mix ratio, accurately weigh the weight of each material, pour the slag, fly ash, aggregate, and mix into a mixer, and stir at a low speed for 2 minutes; slowly add the alkali activator and stir at a low speed for 1 minute; then add water and retarder and stir at a low speed for 1 minute; then add PE fibers. Since the fibers are prone to agglomeration during the mixing process, which affects the uniform dispersion of the fibers in the matrix, it is necessary to manually disperse the blown fibers. Add while stirring, stir at low speed for 3 minutes; take a small part of the fresh gelling material out of the pot for fluidity test, and quickly put the other part into the mold brushed with engine oil in advance, turn on the vibration table, and vibrate while putting it into the mold. The purpose is to reduce the number of bubbles and make the gel more compact. The vibration time is 2 minutes, and the surface of the specimen is smoothed with a knife; after the specimen is formed, it is covered with plastic wrap and moved to the curing site. After curing at room temperature (20±2℃) for 24 hours, the mold is removed, and then the specimens are numbered. The numbered specimens are placed in a water tank for continued curing until 28 days, taken out and dried, and the subsequent experimental process is carried out.

[0105] 4. Lightweight and high-strength EGC fluidity test

[0106] According to the specification "Test method for fluidity of cement mortar" (GB / T 2419-2005), the jumping table test was used to determine the fluidity of LWHS-EGC.

[0107] Table 16 Liquidity of LWHS-EGC

[0108]

[0109] Figure 2 (a) shows the effect of aggregate type on mortar fluidity, and (b) shows the effect of HGM40 volume percentage on mortar fluidity. The results show that the working performance of all groups can meet the requirements.

[0110] Depend on Figure 2(a) It can be seen that the type of aggregate affects the fluidity of LWHS-EGC. After replacing quartz sand with HGM, the fluidity decreases. When the aggregate is quartz sand, the fluidity is 152mm, which is the highest among all aggregates, about 5mm higher than HGM. The reason is speculated to be that when quartz sand is replaced by HGM, the mass of the mixture becomes lighter, so it is not easy to collapse under vibration, which is ultimately reflected in a decrease in fluidity. When the aggregate is hollow glass beads, the fluidity is basically unchanged, among which the fluidity of HGM60 and HGM40 is 147mm, while the fluidity of HGM20 is slightly lower, at 146.5cm, indicating that the type of HGM has basically no effect on the fluidity, that is, the particle size of HGM has basically no effect on the fluidity. By Figure 2 (b) It can be seen that the effect of the volume proportion of HGM40 on the fluidity of LWHS-EGC. The fluidity first increases and then decreases with the increase of the volume proportion of HGM. In the process of increasing the volume proportion of HGM from 8.6% to 22.6%, the fluidity gradually increases from 142mm to 148mm and reaches a peak at this time. It is speculated that this is because the smooth and closed spherical surface of HGM is conducive to increasing the fluidity of the mixture, thereby increasing the workability of the mixture. In the process of increasing the volume proportion of HGM from 22.6% to 36.8%, the fluidity gradually decreases from 148mm to 138mm. The reason is speculated to be that the hollow structure of HGM causes the density of the mixture to decrease, so it is not easy to collapse under the action of vibration, which is ultimately reflected in the decrease in fluidity.

[0111] 5. Static axial compression performance of lightweight and high-strength geopolymer-based composites

[0112] a. Loading test plan

[0113] The static axial compression test of LWHS-EGC is carried out in accordance with the requirements of the standard "Standard Test Methods for Mechanical Properties of Ordinary Concrete" (ASTM-C39). During the pouring, a cylindrical mold is used to cast a Φ100mm×200mm cylindrical specimen. The static axial compression performance test begins after the standard curing period of 28 days.

[0114] For the above 11 different test groups, the total number of specimens for axial static compression tests using three replicate specimens in each group is 33. The detailed parameters of the specimens are shown in Table 17.

[0115] Table 17 Axial compression specimen design

[0116]

[0117] After the specimens reached 28 days of age under standard curing, the static axial compression test began.

[0118] The specimen was loaded using the MATEST C088-01 voltage servo testing machine, and the TDS-540 high-speed static data acquisition instrument was used to collect data. The testing machine adopted a displacement loading scheme with a loading rate of 0.18 mm / min. It was also set to unload when the load dropped to 80% of the peak load to prevent overpressure damage, which would be unfavorable for subsequent observation of its failure mode.

[0119] b. Failure mode:

[0120] Ordinary concrete without fiber addition will experience brittle failure, with a very short failure time and even accompanied by the explosion and splashing of fragments, while concrete with fiber addition will have better ductility when it fails.

[0121] Figure 3 The failure mode of the LWHS-EGC cylindrical specimen is presented. It can be seen that the cylindrical specimen still has very good integrity. Most of the main cracks can be observed on the surface, and the main cracks mainly show the crack development mode of oblique shear development. Further observation of its failure angle shows that the angle between the main crack of the specimen and the axis direction of the cylinder is basically between 15° and 30°.

[0122] And the figure shows the influence of different HGM40 volume proportions on the failure mode of static axial compression cylindrical specimens. Taking the inclination angle of the shear oblique crack of group 4-2 as the benchmark (marked as orange and blue reference lines in the figure), compared with other groups, it can be seen that as the volume proportion of HGM increases from 8.6% to 36.8% (i.e. from group 4-2 to 4-12), the angle between the cylindrical shear oblique crack and the axial direction of the cylinder becomes smaller and smaller, and the clarity of the shear oblique crack becomes lower and lower, until no obvious main crack can be observed to penetrate the specimen. The last two groups also slowly evolved from oblique shear failure to central bulging failure. The reason for this is that the hollow structure of HGM has a certain energy consumption capacity. As the volume proportion of HGM increases, the energy consumption capacity of LWHS-EGC continues to increase, and the energy is gradually absorbed uniformly by the material, which leads to the continuous decrease in the brittleness of the cylindrical specimen and the improvement of ductility until the main crack cannot be formed.

[0123] c. Stress-strain curve

[0124] Figure 4The static axial compression stress-strain curve of LWHS-EGC is presented. The static axial compression test stress-strain curve reflects the deformation capacity and load bearing capacity of LWHS-EGC. The axial compression stress is obtained by dividing the load of the testing machine by the cross-sectional area of ​​the cylinder, and the axial compression strain value is obtained by dividing the two displacement count values ​​collected by the acquisition instrument by the length of the measuring section of 80 cm and then taking the average value. Among them, (a), (b), (c), (d), (e), (f), (g), (h), (i), (j), (k) are the tensile-strain curves of 0-4, 6-4, 2-4, 4-2, 4-3, 4-4, 4-5, 4-6, 4-8, 4-10 and 4-12 groups respectively (3 specimens).

[0125] It can be seen from the figure that the development of the stress-strain curve of the LWHS-EGC static axial compression test is basically divided into four stages: in the first stage, the curve bends upward and the slope continues to increase, indicating that the elastic modulus will change and increase in the initial stage. The initial stage occurs when the strain increases from 0% to 0.1%; in the second stage, the curve rises and develops to a peak value, and the slope remains unchanged, indicating that in this stage, with the increase of strain, the stress increases very steadily and the elastic modulus remains unchanged; in the third stage, the curve suddenly drops, indicating that the cylinder begins to fail at this stage, and the failure also shows brittleness, and the stress will decrease extremely quickly after failure; in the fourth stage, the curve begins to shake and drop slowly, indicating that after reaching the peak failure, the cylinder is still able to withstand a certain pressure and is not completely out of work. The reason for this may be due to the addition of fibers. In the failure stage of the cylindrical specimen, the fibers can provide it with a very good circumferential constraint to control the development of cracks, so that it does not collapse but can still withstand stress.

[0126] And it can be seen that the peak strain of all specimens exceeded 0.4%, and the highest value reached 0.7%, which is 2-3 times the peak strain of ordinary concrete.

[0127] Table 18 shows the characteristic parameters of the static axial compression test of the LWHS-EGC cylinder, including the axial compressive strength and elastic modulus, and also adds a comparison with density. Among them, the elastic modulus is an important performance parameter to measure the difficulty of elastic deformation of cementitious materials. The calculation method is based on formula 3.1:

[0128] E=(S 2 -S 1 ) / (ε 2 -0.000050) (3.1)

[0129] In the formula: E: represents elastic modulus (MPa), S 2 Indicates the stress value corresponding to 40% peak load, S1 Indicates the stress value corresponding to the axial strain value of 0.00005, ε 2 It represents the axial strain value corresponding to the location.

[0130] Table 18 Summary of characteristic parameters of LWHS-EGC static axial compression test

[0131]

[0132] Based on the above analysis, although HGM with small particle size has a higher density, its higher crushing strength will make the comprehensive mechanical properties of LWHS-EGC slightly higher, and its negative impact on the density of LWHS-EGC is not obvious, so it is more suitable for use in LWHS-EGC.

[0133] Figure 5 The influence of aggregate type on static axial compression performance (the density of the static axial compression test corresponds to the ordinate value on the left, the compressive strength corresponds to the first ordinate on the right, and the elastic modulus compressive strength corresponds to the second ordinate on the right). Figure 5 It can be seen that the volume ratio of HGM40 affects the static axial compression performance of LWHS-EGC.

[0134] In terms of compressive strength, as the volume share of HGM40 increases from 8.6% to 36.8%, the compressive strength of LWHS-EGC continues to decrease from 84.7MPa to 35.1MPa. The reason is that the crushing strength of HGM40 is lower than the compressive strength of the base material. Therefore, HGM40 is equivalent to an artificial defect in LWHS-EGC. As the volume share of HGM40 increases, it is equivalent to an increase in artificial defects in LWHS-EGC, which will inevitably lead to a continuous decrease in compressive strength.

[0135] In terms of elastic modulus and density, the change pattern is basically the same as that of compressive strength. As the volume share of HGM40 increases from 8.6% to 36.8%, the elastic modulus and density of LWHS-EGC continue to decrease. The lower elastic modulus means that it is more prone to deformation, so it can effectively improve the brittleness of the material, making it less likely to break when deformed.

[0136] In terms of material density, its change pattern is basically the same as that of compressive strength. As the volume share of HGM increases from 8.6% to 36.8%, the density of LWHS-EGC increases from 1800kg / m 3 Continue to decrease to 1360kg / m 3 The reason is that the density of HGM40 (0.4g / cm 3 ) is much lower than the compressive strength of the matrix material, so the more HGM40 is added, the lower the density of LWHS-EGC.

[0137] Figure 6 The influence of HGM40 volume ratio on the static axial compression performance (the density of the static axial compression test corresponds to the ordinate value on the left, the compressive strength corresponds to the first ordinate on the right, and the elastic modulus compressive strength corresponds to the second ordinate on the right).

[0138] 6. Static axial tensile properties of lightweight and high-strength geopolymer-based composites

[0139] a. Experimental Design

[0140] The static axial tensile test of LWHS-GEC is carried out in accordance with the requirements of the specification "Test Method for Mechanical Properties of High Ductility Fiber Reinforced Cement-Based Composite Materials" (JC / T2461-2018). During casting, a tensile test mold is used to cast a dumbbell-shaped specimen with a size of 330mm×60mm×13mm. The static axial tensile performance test begins after reaching the standard curing age of 28 days.

[0141] Corresponding to the above 11 different test groups, each group was tested with 3 repeated specimens to ensure the reliability of the test results. The total number of specimens subjected to axial static compression tests was 33. The detailed parameters of the specimens are shown in Table 19.

[0142] Table 19 Statistics of LWHS-EGC static axial tension test specimens

[0143]

[0144] b. Load test

[0145] After the specimen reaches 28 days of age under standard curing, the static axial tensile test is started. The LWHS-EGC static axial tensile test of the present invention is carried out in accordance with the test method required by the specification "Test Method for Mechanical Properties of High Ductility Fiber Reinforced Cement-based Composite Materials" (JC / T2461-2018). The tests are all carried out at the Structural Experimental Center of Guangdong University of Technology. The specimens are loaded with a universal testing machine with a maximum force of 100kN, and the TDS-540 high-speed static acquisition instrument is used to collect data simultaneously. The test machine loading adopts a displacement loading scheme, and the tensile rate is 0.5mm / min.

[0146] Figure 7 The failure modes of axial tensile specimens after loading are presented, and some representative groups are selected for display. The failure morphology of tensile specimens can be characterized by the number of cracks on the surface of the specimen and the width of the cracks. In all groups, the cracks are very evenly distributed in the measurement section, and most of the main cracks are very inconspicuous.

[0147] Figure 7(a) shows the effect of different aggregate types on the static axial tension failure mode of LWHS-EGC. It can be seen that both quartz sand and HGM can form very dense cracks, which verifies the feasibility of using HGM instead of quartz sand to design LWHS-EGC. Figure 7 (b) shows the influence of different volume proportions of HGM40 on the static axial tension failure mode of LWHS-EGC. It can be seen that with the increase of different volume proportions of HGM40, the number of cracks shows a trend of becoming increasingly scarce, indicating that the increase in the volume proportion of HGM40 will generally have a negative impact on the number of cracks.

[0148] Table 20 summarizes the crack parameters of the LWHS-EGC static axial tension specimen based on the 60 mm crack identification section, including the average crack width w c 、Number of cracks c , average crack spacing s c =60000 / N c From the summary results in Table 20, it can be seen that the average crack width of each group of specimens is less than 90 μm, which meets the ECC requirement for crack width.

[0149] In terms of the volume share of HGM40, as the volume share of HGM40 in LWHS-EGC increased from 8.6% to 36.8%, the average number of cracks in the axial tension specimens first increased and then decreased (the peak value was 82 when the volume share of HGM40 was 22.6%, corresponding to groups 4-6), while the average crack width continued to decrease from 80μm to 43μm, so it was divided into two processes for discussion.

[0150] In the process of increasing the volume proportion of HGM40 from 8.6% to 22.6% (i.e. from group 4-2 to group 4-6), the average number of cracks increased from 55 to 88, while the average crack width decreased from 80μm to 57μm. This is because the matrix cracking strength and fiber bridging stress of LWHS-EGC both decreased during this process, and the matrix cracking strength decreased faster than the fiber bridging stress year-on-year (the matrix cracking strength decreased by 54% and the fiber bridging stress decreased by 33%), which resulted in the difference between the two becoming larger and larger. Therefore, the increase in the number of cracks will become easier to achieve than the increase in crack width. Therefore, during the axial tension of this process, LWHS-EGC will give priority to increasing the number of cracks rather than increasing the crack width, which ultimately results in an increase in the average number of cracks and a decrease in the average crack width. And PSH E and PSH S The two pseudo-strain hardening indices increased by 26% and 44% respectively during this process, which also proves that LWHS-EGC is increasingly prone to form saturated cracks during this process.

[0151] In the process of increasing the volume proportion of HGM40 from 22.6% to 36.8% (i.e. from group 4-6 to group 4-12), the average number of cracks began to decrease from 82 to 59, while the average crack width continued to decrease from 57μm to 43μm. This is because the matrix cracking strength of LWHS-EGC remained basically unchanged and the fiber bridging stress continued to decrease by 25%. Therefore, in the axial tension of LWHS-EGC, both the number of cracks and the crack width will decrease. And PSH E and PSH S The two pseudo strain hardening indicators were reduced by 77% and 33% respectively in this process, while PSH S The indicator is getting closer and closer to the minimum threshold of 1.2, which can also prove that it will become increasingly difficult for LWHS-EGC to form saturated cracks in this process.

[0152] In terms of HGM types, as the HGM particle size increases from 45 μm to 60 μm in LWHS-EGC, the average number of cracks in the axial tension specimens decreases from 79 to 55, while the average crack width increases from 62 μm to 76 μm. This is also due to the changes in the matrix cracking strength and fiber bridging stress, which can be discussed in two processes.

[0153] After the HGM particle size increases from 45μm to 50μm (i.e., from HGM60 in the 6-4 group to HGM40 in the 4-4 group), the appearance of the microbeads remains intact, so the increase in HGM particle size will make the crack surface of LWHS-EGC more uneven, so the interface bonding strength is higher, which leads to a higher matrix crack strength, from 2.5MPa to 2.8MPa, but the fiber bridging stress is basically unaffected, so it will become increasingly difficult for LWHS-EGC to form new cracks during the axial tension process, so the number of cracks decreases and the crack width increases. And PSH E and PSH S Both pseudo-strain hardening indices decreased slightly during this process, which also proves that it is more difficult for LWHS-EGC to form saturated cracks during this process.

[0154] After the HGM particle size continues to increase from 50μm to 60μm (i.e., from HGM40 of group 4-4 to HGM20 of group 2-4), it can be seen from the microscopic analysis in the previous chapter that HGM20 has been broken during the pouring and mixing process, so the actual volume proportion of HGM20 in LWHS-EGC is lower than the theoretical value calculated during the mix design, and the bonding strength of the cementitious material itself is higher than the interfacial bonding strength between HGM and the cementitious material. Therefore, the reduction in the actual volume proportion of HGM20 increases the matrix cracking strength, but the fiber bridging stress is basically unaffected, so it will become increasingly difficult for LWHS-EGC to form new cracks during the axial tension of this process, so the number of cracks decreases and the crack width increases. In addition, the two pseudo-strain hardening indicators, PSHE and PSHS, decreased by 36% and 13% respectively during this process, which can also prove that it will be more difficult for LWHS-EGC to form saturated cracks during this process.

[0155] Table 20 Summary of crack parameters of LWHS-EGC static axial tension specimens

[0156]

[0157] Figure 8 The static axial tensile stress-strain curve of LWHS-EGC is presented. The static axial tensile test stress-strain curve reflects the tensile deformation capacity and the ability to withstand tensile load of LWHS-EGC. The axial tensile stress is obtained by dividing the load of the testing machine by the cross-sectional area of ​​the middle of the axial tensile specimen. The axial tensile strain value is obtained by dividing the two displacement count values ​​collected by the acquisition instrument by the measuring section length of 80mm and then taking the average value. Among them, (a), (b), (c), (d), (e), (f), (g), (h), (i), (j), (k) are the tensile-strain curves (3 specimens) of groups 0-4, 6-4, 2-4, 4-2, 4-3, 4-4, 4-5, 4-6, 4-8, 4-10 and 4-12 respectively.

[0158] It can be seen from the figure that the development of the static axial tensile stress-strain curve of LWHS-EGC is basically divided into five stages: the first stage is from the zero point of the curve to the first peak point of the curve, that is, the stage from the beginning of the stress to the first crack of the axial tensile specimen. In this stage, the curve rises quickly and the slope remains unchanged. It is the concrete matrix that is at work, reflecting the stiffness of the concrete, and the occurrence time is very short; the second stage is from the first peak point of the curve to the overall rise of the curve to the first inflection point. In this stage, the curve rises rapidly and linearly, and the slope remains basically unchanged. The concrete matrix has stopped working, and it is the fiber that is working, reflecting the elastic stiffness of the fiber; the third stage is from the first inflection point to the second inflection point of the rising stage of the curve. In this stage, the curve becomes a slow rise, and the slope remains basically unchanged. It is still the fiber that is working, reflecting the elastic stiffness after fiber reinforcement; the fourth stage is the curve from the second inflection point to the limit peak. In this stage, the curve rises faster than the previous stage, and the slope remains basically unchanged, reflecting the limit stiffness of the fiber; the fifth stage is a sudden drop in the curve, indicating that the fiber begins to stop working.

[0159] It can also be seen that the ultimate tensile strain of all specimens exceeded 5%, with the highest value reaching 8%, which all met the ECC requirement for a strain value of 3% and had very excellent ductility.

[0160] Table 21 summarizes the key parameters of the LWHS-EGC static axial tensile test, including the first crack tensile strength, ultimate tensile strength, ultimate tensile stress and strain energy, and adds a comparison with density. Among them, the value of the strain energy density is the area formed by the curve from the origin to the extreme peak point and the horizontal axis, which reflects the energy absorption of the material during the deformation process.

[0161] Table 21 Summary of characteristic parameters of LWHS-EGC static axial tension test

[0162]

[0163] c. Effect of aggregate type on static axial tensile properties of LWHS-EGC

[0164] Fig. 9 The effects of different aggregate types on the static axial tensile properties of LWHS-EGC, including first-crack tensile strength, ultimate tensile strength, ultimate tensile strain and strain energy density, are presented. When HGM replaces quartz sand, the first-crack strength and ultimate tensile strength decrease, while the ultimate tensile strain increases, which is due to the difference in the appearance of HGM and quartz sand.

[0165] In terms of initial crack strength, because HGM has a smooth and closed spherical surface and basically does not react with cementitious materials for hydration, while quartz sand has an irregular shape and many irregular edges and corners on the surface that can be firmly embedded in cementitious materials, the interfacial bonding strength between HGM and cementitious materials is lower than that of quartz sand. Therefore, the initial crack strength of LWHS-EGC with HGM aggregate is lower than that of quartz sand.

[0166] In terms of ultimate tensile strength, due to the difference in appearance between HGM and quartz sand, the friction between the matrix and the fiber of the aggregate type HGM is lower than that of quartz sand, that is, the fiber bridging stress is lower. Since the tensile strength of the fiber used in this study is much higher than the fiber bridging stress between the fiber and LWHS-EGC, the fiber will not break but only pull out, so the fiber bridging stress constitutes the ultimate tensile strength of LWHS-EGC. Therefore, the ultimate tensile strength of LWHS-EGC with HGM as the aggregate type is lower than that of quartz sand.

[0167] In terms of ultimate tensile strain, the interface bonding strength between HGM and cementitious materials is lower than that of quartz sand due to the different appearance of HGM and quartz sand, that is, the matrix cracking strength is lower, making it easier for new cracks to form. Therefore, the ultimate tensile strain of LWHS-EGC with HGM aggregate is higher than that of quartz sand. At the same time, it is noted that the ultimate tensile strain of LWHS-EGC with HGM20 aggregate is significantly lower than that of HGM60 and HGM40 aggregates. From the microscopic analysis in Chapter 3, it can be seen that the actual volume proportion of HGM20 in LWHS-EGC is smaller than the theoretical value in the mix design due to the crushing of HGM20. The bonding strength of the cementitious material itself is higher than the interface bonding strength between HGM and cementitious materials, resulting in a higher matrix cracking strength, so new cracks are more difficult to form, and therefore the ultimate tensile strain is low.

[0168] In addition, in terms of strain energy density, when HGM is used to replace quartz sand, the strain energy density decreases significantly. This is because although the material will have a higher ultimate tensile strain after HGM is used to replace quartz sand, it is still not enough to make up for the gap in the ultimate tensile strength of the material.

[0169] d. Effect of HGM40 volume ratio on static axial tensile properties of LWHS-EGC

[0170] Fig.10The effects of different volume proportions of HGM40 on the static axial tensile properties of LWHS-EGC are presented, including first crack tensile strength, ultimate tensile strength, ultimate tensile strain and strain energy. As the volume proportion of HGM40 increases, the first crack strength, ultimate tensile strength and strain energy density continue to decrease, while the ultimate tensile strain first increases and then decreases, with the peak value being when the volume proportion of HGM is 15.8% (i.e., group 4-4), which is due to the smooth, closed and smooth spherical appearance of HGM.

[0171] In terms of first crack strength, because HGM40 has a smooth, closed and smooth spherical appearance and basically does not undergo hydration reaction with the cementitious material, the interfacial bonding strength between HGM40 and the cementitious material is lower than the bonding strength of the cementitious material itself. Therefore, as the volume share of HGM40 increases, the first crack strength decreases, but because the value itself is small, the decrease is not obvious and is always not less than 2MPa.

[0172] In terms of ultimate tensile strength, because HGM40 has a smooth, closed and smooth spherical appearance, the higher the volume proportion of HGM40 in the matrix, the lower the friction between the matrix and the fiber, that is, the lower the fiber bridging stress, and because the fiber bridging stress constitutes the ultimate tensile strength of LWHS-EGC, the ultimate tensile strength becomes lower and lower with the increase of HGM40 volume proportion. And it can be seen that in the process of increasing the volume proportion of HGM40 from 8.6% to 15.8%, the ultimate tensile strength decreases from 7.78MPa to 7.46MPa, which decreases very slowly and has basically no negative impact on the ultimate tensile strength of the material; in the process of increasing the volume proportion of HGM40 from 15.8% to 36.8%, the ultimate tensile strength suddenly drops sharply from 7.46MPa to 5.76MPa, and then continues to slowly decrease to 4.64MPa, which has a more obvious negative impact on the ultimate tensile strength of the material.

[0173] In terms of ultimate tensile strain, when the volume proportion of HGM40 increased from 8.6% to 15.8%, the ultimate tensile strain increased from 7.41% to 8.19%. This is because the appearance characteristics of HGM make the interfacial bonding strength between HGM and cementitious materials lower than the bonding strength of the cementitious materials themselves. This leads to the higher the volume proportion of HGM, the lower the matrix cracking strength, which also makes it easier for new cracks to form, and from PSH E and PSH SThe continuous improvement of these two pseudo-strain hardening indicators in this process also shows that it is becoming easier to form saturated cracks. As the volume proportion of HGM continued to increase from 15.8% to 36.8%, the ultimate tensile strain began to slowly decrease from 8.19% to 5.39%, but its value still reached more than 5%. This is because the interfacial bonding strength between HGM and cementitious materials remained basically unchanged during this process, while the fiber bridging stress continued to decrease, so both the number of cracks and the crack width would decrease, which in turn led to a decrease in the ultimate tensile strain and a decrease in the PSH. E and PSH S The two pseudo-strain hardening indicators continue to decrease in this process, which also shows that it is becoming increasingly difficult to form saturated cracks. This means that if the project mainly requires the ultimate tensile strain of LWHS-EGC, the volume proportion of HGM can be appropriately increased to achieve a lighter weight.

[0174] In terms of strain energy density, as the volume share of HGM40 increases, the strain energy density first fluctuates and then decreases significantly. In the process of HGM volume share increasing from 8.6% to 15.8%, the strain energy density increases from 35kJ / m 3 Up to 40kJ / m 3 The reason is that in this process, the ultimate tensile strain of the material increases, but the ultimate tensile strength decreases at the same time, and the effects of the two on the strain energy offset each other; in the process where the volume proportion of HGM continues to increase from 15.8% to 36.8%, the strain energy begins to decrease significantly. The reason is that in this process, the ultimate tensile strength and the ultimate tensile stress are both decreasing at the same time, and the effects of the two on the strain energy are superimposed, resulting in a significant reduction in strain energy.

[0175] 7. Dynamic compression performance of lightweight and high-strength geopolymer-based composites

[0176] a. Experimental Design

[0177] The dynamic compression test of LWHS-GEC is carried out in accordance with the requirements of the specification "High Strain Rate Room Temperature Compression Test Method for Materials" (GB / T34108-2017). During casting, a dynamic compression mold is used to cast a cylindrical specimen with a size of Ф100mm×50mm. The dynamic compression performance test begins after reaching the standard curing age of 28 days.

[0178] For 11 different test groups, each impact air pressure of each group was tested with 3 repeated specimens to ensure the reliability of the test results. Each group was set with four air pressure values ​​of 0.4MPa, 0.5MPa, 0.6MPa and 0.7MPa. The total number of specimens for axial static compression test was 132. The detailed parameters of the specimens are shown in Table 22.

[0179] Table 22 Statistics of LWHS-EGC dynamic compression test specimens

[0180]

[0181] b. Test methods

[0182] After the specimens reached 28 days of age under standard curing, the dynamic compression test began.

[0183] c. Failure mode

[0184] The specimens can be divided into four types according to the degree of failure. The first failure type is when the strain rate is 50s -1 to 75s -1 The second failure mode is when the strain rate increases to 90s. -1 to 115s -1 When the strain rate increases to 140s, the specimen cracks and separates into several parts of different sizes, but there is a main part, and the cracked and separated parts are mostly located around the specimen. The third failure mode is when the strain rate continues to increase to 140s -1 to 165s -1 When the strain rate increases to 190s, the specimen is broken. The main part of the specimen can no longer be found, but it has become fragments, but mainly large fragments, and there are fewer small fragments. The fourth failure mode is when the strain rate increases to 190s -1 When the strain rate is above 0.05, the specimen is severely broken, and the specimen becomes mainly small fragments, with few large fragments, and powder begins to be produced. This is because when the strain rate increases, the bullet actually has a greater initial velocity, so the impact energy provided increases accordingly, but the concrete cannot transfer such a large amount of energy in a short time, so it must consume energy through crack expansion, absorb it and release it in a short time, and the crack will develop to the weak interface transition zone of the concrete. If the energy received by the specimen in a short time is too large and not enough to consume this part of the energy through crack expansion, more new cracks will be formed to consume energy. Because compared with crack expansion, the formation and initiation of new cracks requires more energy.

[0185] After replacing quartz sand with HGM, the strain rate is 50s -1 to 165s -1 When the strain rate exceeds 190s, the damage degree of LWHS-EGC with HGM aggregate is more serious. This is because the hollow thin-walled structure of HGM leads to lower compressive strength of LWHS-EGC, so it is less likely to resist damage. -1Finally, the particle size of LWHS-EGC fragments with HGM aggregate type is larger. This is because the hollow thin-wall structure of HGM makes the LWHS-EGC material itself have a stronger energy absorption capacity, so there is no need to generate more new cracks to absorb energy.

[0186] As the volume proportion of HGM40 in LWHS-EGC increases, the strain rate increases at 50s -1 to 165s -1 When the strain rate exceeds 190s, the damage degree of LWHS-EGC becomes more and more serious, because its compressive strength is lower and it is less likely to resist damage; -1 After that, the particle size of LWHS-EGC fragments becomes larger and larger. This is because the larger the volume share of HGM40, the stronger the energy absorption capacity of LWHS-EGC material itself. Therefore, the difference in the degree of fragmentation of each group of LWHS-EGC is essentially caused by the hollow thin-walled structure of HGM.

[0187] d. Stress-strain curve

[0188] Fig.11 The dynamic compression test stress-strain curve of LWHS-EGC is presented, which reflects the impact deformation capacity and the ability to withstand impact load of LWHS-EGC. Among them, (a), (b), (c), (d), (e), (f), (g), (h), (i), (j), and (k) are the tensile-strain curves of 0-4, 6-4, 2-4, 4-2, 4-3, 4-4, 4-5, 4-6, 4-8, 4-10, and 4-12 groups, respectively.

[0189] It can be seen from the figure that the development of the stress-strain curve of the LWHS-EGC dynamic compression test is basically divided into three stages: the first stage is from the zero point of the curve to the first peak of the curve. In this stage, the curve rises quickly and the time is very short. With the increase of the volume proportion of HGM40, its slope tends to decrease, and the strain corresponding to the peak tends to increase; the second stage is from the first peak of the curve to the stage of up and down fluctuations at the peak. Different groups have different fluctuation forms, and the time of this stage is quite different for different groups; the third stage is from the end of the curve shaking to the stage of rapid decline to the bottom of the valley. Different groups have different decline forms in this stage.

[0190] Tables 23 and 24 present a summary of the characteristic parameters of the dynamic compression test of LWHS-EGC, including peak stress at no strain rate, dynamic impact toughness and dynamic growth factor (DIF). The value of dynamic impact toughness is the sum of the area of ​​the rising section of the dynamic stress-strain curve and the area before 80% of the peak stress in the descending section. The dynamic growth factor is the ratio of the dynamic compression peak stress to the static compression peak stress, and the strain rate is taken as the average strain rate.

[0191] Table 23 Summary of characteristic parameters of LWHS-EGC dynamic compression test for different aggregate types

[0192]

[0193] Table 24 Summary of the results of dynamic impact tests of LWHS-EGC with different volume ratios of HGM

[0194]

[0195]

[0196] Fig.12 The effect of aggregate type on the dynamic compression properties of LWHS-EGC is presented.

[0197] In terms of dynamic compressive strength and DIF, the dynamic compressive strength and DIF of LWHS-EGC increase with the increase of strain rate, showing an obvious strain rate effect. After HGM replaces quartz sand, the slope increases, indicating that HGM can improve the strain rate sensitivity of LWHS-EGC. -1 Increased to 213s -1 , its dynamic compressive strength increased from 119MPa to 154MPa, and its DIF increased from 1.099 to 1.422, an increase of 29%. -1 Increase to 190s -1 Its dynamic compressive strength increased from 77MPa to 112MPa, and its DIF increased from 1.004 to 1.456, an increase of 45%. -1 Increase to 215s -1 Its dynamic compressive strength increased from 78MPa to 114MPa, and its DIF increased from 1.086 to 1.588, an increase of 46%. -1 Increased to 209s -1, its dynamic compressive strength increased from 86MPa to 121MPa, and its DIF increased from 1.079 to 1.528, an increase of 42%. The strain rate affects the performance of the material because there is a time relationship between the impact load and the damage to the material. Under the impact load of high strain rate, the internal damage of the concrete cannot occur immediately in a short time, resulting in delayed damage. This explains the high strain rate sensitivity of LWHS-EGC with HGM aggregate. Because HGM has a hollow thin-walled structure, it can enhance the deformation capacity of LWHS-EGC more than quartz sand, which aggravates its delayed damage phenomenon under high strain rate.

[0198] In terms of impact toughness, the impact toughness of LWHS-EGC also increases with the increase of strain rate, showing a significant strain rate effect. After replacing quartz sand with HGM, the impact toughness of LWHS-EGC decreases. -1 Increased to 213s -1 , its impact toughness ranges from 0.919MJ / m 3 Increased to 1.251MJ / m 3 , an increase of 36%. For LWHS-EGC with HGM60 aggregate, as the strain rate increases from 52s -1 Increase to 190s -1 , its impact toughness ranges from 0.615MJ / m 3 Increased to 0.918MJ / m 3 , an increase of 49%. For LWHS-EGC with HGM40 aggregate, as the strain rate increases from 61s -1 Increase to 215s -1 , its impact toughness ranges from 0.499MJ / m 3 Increased to 1.091MJ / m 3 , an increase of 115%. For LWHS-EGC with HGM20 aggregate, as the strain rate increases from 63s -1 Increased to 209s -1 , its impact toughness ranges from 0.652MJ / m 3 Increased to 1.059MJ / m 3, an increase of 63%. Impact toughness is calculated based on the area enclosed by the dynamic stress-strain curve. It mainly depends on the maximum stress and its corresponding strain in the dynamic stress-strain curve. It reflects the ability of the material to absorb energy from the impact load to the failure. It is a comprehensive reflection of the deformation capacity and strength of concrete after being loaded. The lower strength of HGM itself and its weaker bonding strength with the matrix reduce the cracking load of LWHS-EGC, thereby reducing its dynamic compressive strength. Although HGM can enhance the deformation capacity of LWHS-EGC, it still cannot make up for the negative impact of the decrease in dynamic compressive strength on impact toughness.

[0199] Fig.13 The effect of HGM40 volume ratio on the dynamic compression performance of LWHS-EGC is presented.

[0200] In terms of dynamic compressive strength and DIF, the dynamic compressive strength and DIF of LWHS-EGC increase with the increase of strain rate, showing an obvious strain rate effect. However, as the volume proportion of HGM increases from 8.6% to 36.8%, the slope decreases continuously, indicating that excessive HGM will reduce the strain rate sensitivity of LWHS-EGC. -1 Increased to 163s -1 Its dynamic compressive strength increased from 87MPa to 163MPa, and its DIF increased from 1.071 to 1.606, an increase of 50%. For LWHS-EGC with a volume proportion of HGM40 of 12.3%, as the strain rate increased from 60s -1 Increased to 167s -1 Its dynamic compressive strength increased from 81MPa to 108MPa, and its DIF increased from 1.126 to 1.503, an increase of 33%. For LWHS-EGC with a volume proportion of 15.8% HGM40, as the strain rate increased from 61s -1 Increase to 215s -1 Its dynamic compressive strength increased from 78MPa to 114MPa, and its DIF increased from 1.086 to 1.588, an increase of 46%. For LWHS-EGC with a volume proportion of 19% HGM40, as the strain rate increased from 61s -1 Increase to 215s -1 Its dynamic compressive strength increased from 73MPa to 108MPa, and its DIF increased from 1.071 to 1.571, an increase of 47%. For LWHS-EGC with a volume proportion of HGM40 of 22.6%, as the strain rate increased from 60s -1 Increased to 239s -1Its dynamic compressive strength increased from 65MPa to 102MPa, and its DIF increased from 1.044 to 1.637, an increase of 57%. For LWHS-EGC with HGM40 volume accounting for 28%, as the strain rate increased from 63s -1 Increased to 192s -1 Its dynamic compressive strength increased from 58MPa to 75MPa, and its DIF increased from 1.039 to 1.350, an increase of 30%. For LWHS-EGC with a volume proportion of 32.7% HGM40, as the strain rate increased from 59s -1 Increased to 211s -1 Its dynamic compressive strength increased from 47MPa to 60MPa, and its DIF increased from 1.025 to 1.315, an increase of 28%. For LWHS-EGC with a volume proportion of 36.8% HGM40, as the strain rate increased from 57s -1 Increased to 221s -1 , its dynamic compressive strength increased from 37MPa to 46MPa, and its DIF increased from 1.065 to 1.307, an increase of 23%. This is because HGM has a smooth and closed spherical surface and basically does not react with the matrix, so the interfacial bonding strength with the matrix is ​​low, which has an adverse effect on the interface performance of LWHS-EGC, and the damage is accelerated under impact load, which leads to a reduction in the delayed damage of LWHS-EGC at high strain rates, thereby reducing the strain rate sensitivity of LWHS-EGC.

[0201] In terms of impact toughness, the impact toughness of LWHS-EGC also increases with the increase of strain rate, showing a significant strain rate effect. However, as the volume proportion of HGM increases from 8.6% to 36.8%, the slope decreases until there is basically no strain rate effect. -1 Increased to 163s -1 , its impact toughness ranges from 0.932MJ / m 3 Increased to 1.939MJ / m 3 , an increase of 108%; LWHS-EGC with HGM40 volume proportion of 12.3%, as the strain rate increases from 60s -1 Increased to 167s -1 , its impact toughness ranges from 0.474MJ / m 3 Increased to 0.892MJ / m 3 , an increase of 88%; LWHS-EGC with HGM40 volume proportion of 15.8%, as the strain rate increases from 61s -1 Increase to 215s -1 , its impact toughness ranges from 0.499MJ / m 3Increased to 1.071MJ / m 3 , an increase of 115%; LWHS-EGC with HGM40 volume proportion of 19%, as the strain rate increases from 61s -1 Increase to 215s -1 , its impact toughness ranges from 0.436MJ / m 3 Increased to 1.500MJ / m 3 , an increase of 244%; LWHS-EGC with HGM40 volume proportion of 22.6%, as the strain rate increases from 60s -1 Increased to 239s -1 As the strain rate increases from 61s -1 Increase to 215s -1 , its impact toughness ranges from 0.602MJ / m 3 Increased to 0.975MJ / m 3 , an increase of 62%; LWHS-EGC with HGM40 volume accounting for 28%, as the strain rate increases from 63s -1 Increased to 192s -1 As the strain rate increases from 61s -1 Increase to 215s -1 , its impact toughness ranges from 0.360MJ / m 3 Increased to 0.223MJ / m 3 , the increase is -38%; LWHS-EGC with HGM40 volume proportion of 32.7%, as the strain rate increases from 61s -1 Increase to 215s -1 , its impact toughness ranges from 0.143MJ / m 3 Increased to 0.320MJ / m 3 , an increase of 124%; LWHS-EGC with HGM40 volume proportion of 36.8%, as the strain rate increases from 57s -1 Increased to 221s -1 , as the strain rate increases from 61s -1 Increase to 215s -1 , its impact toughness ranges from 0.204MJ / m 3 Increased to 0.264MJ / m 3 , an increase of 30%. This is because the low strength of HGM itself and the relatively weak interface bonding strength with the matrix work together to greatly reduce the cracking load of LWHS-EGC, thereby greatly reducing its dynamic compressive strength. Although HGM can enhance the deformation capacity of LWHS-EGC, it still cannot make up for the negative impact toughness caused by the decrease in dynamic compressive strength.

[0202] The above-described embodiments are merely descriptions of preferred embodiments of the present invention and are not intended to limit the scope of the present invention.

Claims

1. A lightweight and high-strength geopolymer-based composite material, characterized in that: The raw materials consist of the following components: Hollow glass microspheres, PE fibers, slag, fly ash, alkali activator, retarder and water; Wherein, the volume proportion of the hollow glass microspheres in the raw material is 8.6%-36.8%; The volume proportion of the PE fiber in the raw material is 2%.

2. The lightweight and high-strength geopolymer-based composite material according to claim 1, characterized in that: The density of the hollow glass microspheres is 0.2-0.6 g / cm 3 , the compressive strength is 10-55MPa.

3. The lightweight and high-strength geopolymer-based composite material according to claim 1, characterized in that: The particle size of the hollow glass microspheres is 45-60 μm.

4. The lightweight and high-strength geopolymer-based composite material according to claim 1, characterized in that: The alkaline activator is prepared by mixing a 2.25 modulus sodium silicate solution and a 10 mol / L sodium hydroxide solution in a mass ratio of 2:

1.

5. The lightweight and high-strength geopolymer-based composite material according to claim 4, characterized in that: The raw material ratio is as follows: Fly ash 406-586.8kg / m 3 , slag 406-586.8kg / m 3 , hollow glass microspheres 35.4-147.3kg / m 3 , sodium hydroxide solution 108.4-149.8kg / m 3 , sodium silicate solution 216.9-312.9kg / m 3 , water 48.7-70.3kg / m 3 , retarder 8.1-11.7kg / m 3 , PE fiber 19.4kg / m 3 .

6. The method for preparing a lightweight and high-strength geopolymer-based composite material according to any one of claims 1 to 5, characterized in that: The raw materials are mixed evenly to prepare the lightweight and high-strength geopolymer-based composite material.

Citation Information

Patent Citations

  • Inorganic gel matrix composite foam material and preparation method thereof

    CN107098668A

  • Ultra-light high-strength geopolymer-based composite material and preparation method thereof

    CN116903390A

  • Geopolymer composite and geopolymer matrix composition

    WO2017070748A1