Quick-setting paste material, preparation method and application
By using the paste material preparation method of components such as coal gangue and gasification slag in coal mining, the problems of long coagulation time and low early strength of the paste material are solved, rapid coagulation and high durability are achieved, and cost is reduced. Meets the liquidity and strength requirements of coal mine filling.
Patent Information
- Application Number
- CN202411018409.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
The existing paste materials have been set for too long in coal mining and have too low early strength, which affects the production efficiency of coal mines. The existing method for preparing quick-greasing paste materials increases material costs and leads to structural defects, affecting durability.
Using coal gangue, coal gasification slag, cement, fly ash, magnesium slag, sodium bicarbonate and quick-setting agent, the proportion and particle size distribution of material components are controlled through the agitation preparation method, and early hydration reactions are promoted. Reactions are made to generate a filler gel to enhance material density and durability.
It realizes rapid condensation and high early strength of paste materials, reduces material costs, improves the durability and compactness of materials, and meets the fluidity and strength requirements of coal mine filling.
Smart Images

Figure CN118930143A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of coal mining, and in particular relates to a quick-setting paste material, a preparation method and an application thereof. Background Art
[0002] Backfill mining is an effective way to solve ecological environmental damage such as surface subsidence and soil erosion. The post-backfilling process currently used is not mature enough due to the related filling process. In particular, the setting time of the paste material used for filling is too long and the early strength is too low, which makes it impossible for the hydraulic support to move the frame in time, thus affecting the mining progress and resulting in low coal mine production efficiency. The existing method for preparing quick-setting paste materials is to increase the cement content, water reducer content and quick-setting agent content. This method not only greatly increases the cost of the material, but also due to the early hydration reaction of the material, the skeleton is fixed, which hinders the further hydration reaction of the cement material in the later stage, resulting in a large number of structural defects in the quick-setting paste material, and the later strength improvement is small, which is not conducive to the durability of the material. It is in urgent need of improvement. Summary of the invention
[0003] In view of the defects and shortcomings of the prior art, the purpose of the present invention is to provide a quick-setting paste material, a preparation method and an application thereof, so as to solve the technical problems in the prior art of long setting time and low early strength of the paste material for post-frame filling.
[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:
[0005] A method for preparing a quick-setting paste material, the method comprising the following steps:
[0006] Step 1: Pour coal gangue and coal gasification slag into a stirring device, add water into the stirring device, mix and stir at a rate of 100 to 200 r / min for 1 to 3 minutes to obtain a mixed material A.
[0007] Step 2: Add cement, fly ash, magnesium slag, water reducer and water to the mixed material A in sequence, mix and stir at a rate of 100 to 200 r / min for 3 to 5 minutes to obtain slurry B;
[0008] Step 3, adding sodium bicarbonate and accelerating agent to slurry B, mixing and stirring at a rate of 100 to 200 r / min for 3 to 5 minutes, to obtain a quick-setting paste material;
[0009] The quick-setting paste material comprises the following components in parts by weight: 100-200 parts of cement, 100-200 parts of fly ash, 50-100 parts of magnesium slag, 150-300 parts of coal gasification slag, 60-1200 parts of coal gangue, 8-16 parts of sodium bicarbonate, 0.2-1.0 parts of water reducing agent, 2-10 parts of quick-setting agent and 200-350 parts of water.
[0010] The present invention also has the following technical features:
[0011] Specifically, the accelerating setting agent is selected from one or more of sodium aluminate, aluminum sulfate, calcium sulfoaluminate and sodium sulfate.
[0012] Furthermore, the water reducer is selected from one or more of polycarboxylate water reducers and naphthalene water reducers.
[0013] Furthermore, at least 80% of the fly ash powder particle size is less than 45 μm; the particle size of the magnesium slag is less than 75 μm, the particle size of the coal gasification slag aggregate is 0.075 mm to 4.75 mm, and the particle size of the coal gangue aggregate is less than 20 mm.
[0014] Furthermore, the method comprises the following steps:
[0015] Step 1: Pour coal gangue and coal gasification slag into a stirring device, add water into the stirring device, mix and stir at a rate of 100 r / min for 2 minutes to obtain a mixed material A.
[0016] Step 2: Add cement, fly ash, magnesium slag, water reducer and water to the mixture A in sequence, mix and stir at a rate of 200 r / min for 3 minutes to obtain slurry B;
[0017] Step 3, adding sodium bicarbonate and accelerating agent to slurry B, mixing and stirring at a rate of 200 r / min for 5 minutes, to obtain a quick-setting paste material;
[0018] The quick-setting paste material comprises the following components by weight: 150 parts of cement, 150 parts of fly ash, 70 parts of magnesium slag, 200 parts of coal gasification slag, 1200 parts of coal gangue, 15 parts of sodium bicarbonate, 0.8 parts of water reducing agent, 6 parts of quick-setting agent and 260 parts of water.
[0019] The present invention also protects a quick-setting paste material, which is prepared by the above-mentioned preparation method.
[0020] Furthermore, the setting time of the paste material is less than 3 hours, the 1d compressive strength is greater than 2MPa, and the 28d compressive strength is greater than 5MPa.
[0021] The present invention also protects the application of the quick-setting paste material in filling mining.
[0022] Compared with the prior art, the present invention has the following beneficial technical effects:
[0023] (1) The quick-setting paste material provided by the present invention is a cementitious material, and a large amount of solid waste materials are used in the preparation of raw materials, which can effectively reduce costs; there are a large number of spherical particles in the coal gasification slag particles, which can replace part of the gangue in an appropriate amount, thereby improving the workability of the material, enhancing the fluidity of the slurry, increasing the uniformity of the distribution of each component after the material is solidified, and reducing the use of water reducers; the coal gasification slag phase is mainly glassy aluminosilicate, which is added to the cement-based paste material and further reacts with the cement hydration product calcium hydroxide to generate additional hydrated calcium silicate gel, which fills the internal defects of the stone body and increases the density of the stone body, thereby improving the durability of the material.
[0024] (2) The quick-setting paste material provided by the present invention can be used for mining and filling. The quick-setting agent added to the paste material can promote the early hydration reaction of cement, generate hydration products while consuming a large amount of mixing water, increase the internal density of the material, reduce the fluidity of the paste, shorten the material setting time, and improve the early strength of the material; the added magnesium slag further reacts with the carbon dioxide in the system to generate a large amount of calcium carbonate, magnesium carbonate and silica gel, which fill the gaps in the early material, increase the density of the material, and improve the early strength of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a particle morphology diagram of the coal gasification slag used in Example 1;
[0026] Figure 2 (a) is a scanning electron microscope image of the quick-setting paste material prepared in Example 1;
[0027] Figure 2 (b) is the energy spectrum of the quick-setting paste material obtained in Example 1;
[0028] Figure 3 This is a scanning electron microscope image of the quick-setting paste material prepared in Comparative Example 1;
[0029] Figure 4 This is a scanning electron microscope image of the quick-setting paste material prepared in Comparative Example 2;
[0030] Figure 5 This is a scanning electron microscope image of the morphology of coal gasification furnace slag inside the quick-setting paste material prepared in Example 1.
[0031] The technical solution of the present invention is further described below in conjunction with embodiments. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by any ordinary technician in the field belong to the scope of protection of the present invention.
[0033] It should be noted that all raw materials in the present invention, unless otherwise specified, are raw materials known in the art.
[0034] The technical concept of the present application is: introducing magnesium slag, coal gasification slag, sodium bicarbonate, sodium aluminate and aluminum sulfate and other components, so that the materials can synergistically undergo secondary reactions after the hydration reaction in the early stage, and generate a large number of reaction products to fill in the early structural defects, thereby reducing material costs and ensuring material performance. Specifically, the following aspects are discussed: using coal gasification slag as aggregate, the particle size of the coal gasification slag is between 0.075mm and 4.75mm, and most of them are spherical particles. The introduction of an appropriate amount not only increases the fine aggregate content of the system, but also the spherical particles can reduce the friction of the particles inside the slurry, increase the workability of the material and the fluidity of the slurry, and reduce the amount of water reducer, so that the components are dispersed more evenly to form a more homogeneous whole; by introducing an accelerator to promote the early hydration reaction of cement, the paste material has early strength properties; the added accelerator reacts with the sodium bicarbonate in the component The reaction releases carbon dioxide: Al2(SO4)3+NaHCO3→Al(OH)3↓+CO2↑+Na2SO4, and the carbon dioxide reacts with the magnesium slag in the system as follows: C2S+2CO2→2CaCO3+SiO2(gel), CaO+CO2→CaCO3↓, MgO+CO2→MgCO3↓. These products further fill the structural voids in the early hydration products of cement under the action of the accelerator sodium aluminate, which are mainly composed of ettringite. The silica gel generated by the carbonization reaction of the magnesium slag reacts with the calcium hydroxide in the cement hydration products as follows: SiO2(gel)+Ca(OH)2+H2O→CSH(gel). Under the action of calcium hydroxide, the silica gel is converted into CSH gel with stronger gelling properties, making the structure denser and improving the compressive strength.
[0035] The components of the coal gangue, fly ash, coal gasification slag and magnesium slag used in the present invention are shown in Tables 1 to 4:
[0036] <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> <![CDATA[Na2O]]> MgO CaO <![CDATA[K2O]]> <![CDATA[TiO2]]> LOSS 55.55 19.75 11.15 4.61 3.17 1.79 1.10 0.62 2.26
[0037] Table 1. Chemical composition of coal gangue (%)
[0038] <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> CaO MgO <![CDATA[Na2O]]> <![CDATA[SO3]]> <![CDATA[TiO2]]> LOSS 35.11 16.80 4.43 22.62 2.47 0.93 15.32 0.55 1.77
[0039] Table 2. Chemical composition of fly ash (%)
[0040] <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO <![CDATA[Fe2O3]]> MgO <![CDATA[SO3]]> LOSS 46.59 26.65 16.21 5.38 1.60 0.04 0.61
[0041] Table 3. Chemical composition of coal gasification slag (%)
[0042] <![CDATA[SiO2]]> <![CDATA[Al2O3]]> CaO <![CDATA[Fe2O3]]> MgO <![CDATA[SiO2]]> LOSS 29.88 1.06 50.98 3.52 11.27 29.88 3.29
[0043] Table 4. Chemical composition of magnesium slag (%)
[0044] In accordance with the above technical scheme, specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical scheme of this application fall within the protection scope of the present invention.
[0045] Example 1
[0046] This embodiment provides a method for preparing a quick-setting paste material, the method comprising the following steps:
[0047] Step 1: Pour coal gangue and coal gasification slag into a stirring device, add water into the stirring device, mix and stir at a rate of 100 r / min for 2 minutes to obtain a mixed material A.
[0048] Step 2: Add cement, fly ash, magnesium slag, water reducer and water to the mixture A in sequence, mix and stir at a rate of 200 r / min for 3 minutes to obtain slurry B;
[0049] Step 3, adding sodium bicarbonate and accelerating agent to slurry B, mixing and stirring at a rate of 200 r / min for 5 minutes, to obtain a quick-setting paste material;
[0050] The accelerating agents used in this embodiment are sodium aluminate and aluminum sulfate, and the water reducing agent is a polycarboxylate water reducing agent.
[0051] The quick-setting paste material includes the following components in parts by weight: 150 parts of cement, 150 parts of fly ash, 70 parts of magnesium slag, 200 parts of coal gasification slag, 1200 parts of coal gangue, 15 parts of sodium bicarbonate, 0.8 parts of polycarboxylate water reducer, 4.5 parts of sodium aluminate, 1.5 parts of aluminum sulfate and 260 parts of water.
[0052] At least 80% of the fly ash powder particle size is less than 45 μm; the magnesium slag particle size is less than 75 μm, the coal gasification slag aggregate particle size is 0.075 mm to 4.75 mm, and the coal gangue aggregate particle size is less than 20 mm.
[0053] The performance of the quick-setting paste material prepared in this example was tested, and the results are shown in Table 5.
[0054] The scanning electron microscope image of the quick-setting paste material prepared in this embodiment is as follows: Figure 2 (a) shows the energy spectrum of the quick-setting paste material. Figure 2 (b) as shown.
[0055] The quick-setting paste material prepared in this embodiment can be used for mining and filling behind the frame of the coal mining face. During filling, the prepared quick-setting paste material is transported to the coal mining face by the filling pump through the pipeline. A bag of a certain size is arranged behind the hydraulic support of the coal mining face. According to the specific coal mining process requirements, a material distribution port can be set every several supports. When the material is transported from the ground to the working face, the flow pump is turned on to control the conveying rate to fill the quick-setting agent and the paste material into the bag arranged behind the hydraulic support until the frame is full and the top is formed. According to the on-site working conditions, the filling base paste can be prepared with other components first, and then during the filling process, the quick-setting agent of the formula amount can be added to the filling base paste.
[0056] Example 2
[0057] The preparation method steps used in this embodiment are the same as those in Example 1, except that the ratio of the raw material components is different. In this embodiment, the quick-setting paste material includes the following components by weight: 100 parts of cement, 100 parts of fly ash, 50 parts of magnesium slag, 200 parts of coal gasification slag, 1200 parts of coal gangue, 10 parts of sodium bicarbonate, 0.53 parts of water reducer, 3.0 parts of sodium aluminate, 1.0 parts of aluminum sulfate, and 175 parts of water. In this embodiment, a quick-setting paste material is finally prepared.
[0058] The performance of the quick-setting paste material prepared in this example was tested, and the results are shown in Table 5.
[0059] Example 3
[0060] The preparation method steps used in this embodiment are the same as those in Example 1, except that the ratio of the raw material components is different. In this embodiment, the quick-setting paste material includes the following components by weight: 200 parts of cement, 200 parts of fly ash, 100 parts of magnesium slag, 200 parts of coal gasification slag, 1200 parts of coal gangue, 20 parts of sodium bicarbonate, 1.0 part of water reducer, 6.0 parts of sodium aluminate, 2.0 parts of aluminum sulfate, and 350 parts of water. In this embodiment, a quick-setting paste material is finally prepared.
[0061] The performance of the quick-setting paste material prepared in this example was tested, and the results are shown in Table 5.
[0062] Comparative Example 1
[0063] The preparation method steps used in this comparative example are the same as those in Example 1, with the only difference being that the raw material components do not contain magnesium slag. In this comparative example, the quick-setting paste material comprises the following components in parts by weight: 150 parts of cement, 220 parts of fly ash, 200 parts of coal gasification slag, 1200 parts of coal gangue, 15 parts of sodium bicarbonate, 0.8 parts of water reducer, 4.5 parts of sodium aluminate, 1.5 parts of aluminum sulfate, and 260 parts of water.
[0064] The performance of the quick-setting paste material prepared in this comparative example was tested, and the results are shown in Table 5.
[0065] Comparative Example 2
[0066] The preparation method steps used in this comparative example are the same as those in Example 1, except that aluminum sulfate is not contained. In this comparative example, the quick-setting paste material comprises the following components in parts by weight: 150 parts of cement, 150 parts of fly ash, 70 parts of magnesium slag, 200 parts of coal gasification slag, 1200 parts of coal gangue, 15 parts of sodium bicarbonate, 0.8 parts of water reducer, 4.5 parts of sodium aluminate, and 260 parts of water.
[0067] The performance of the quick-setting paste material prepared in this comparative example was tested, and the results are shown in Table 5.
[0068] Comparative Example 3
[0069] The preparation method steps used in this comparative example are the same as those in Example 1, except that no coal gasification slag is contained. In this comparative example, the quick-setting paste material comprises the following components in parts by weight: 150 parts of cement, 150 parts of fly ash, 70 parts of magnesium slag, 1400 parts of coal gangue, 15 parts of sodium bicarbonate, 0.8 parts of water reducer, 4.5 parts of sodium aluminate, 1.5 parts of aluminum sulfate, and 260 parts of water.
[0070] The performance of the quick-setting paste material prepared in this comparative example was tested, and the results are shown in Table 5.
[0071] Comparative Example 4
[0072] The preparation method steps used in this comparative example are the same as those in Example 1, except that sodium bicarbonate is not contained. In this comparative example, the quick-setting paste material comprises the following components in parts by weight: 150 parts of cement, 150 parts of fly ash, 70 parts of magnesium slag, 200 parts of coal gasification slag, 1200 parts of coal gangue, 0.8 parts of water reducer, 4.5 parts of sodium aluminate, 1.5 parts of aluminum sulfate, and 260 parts of water.
[0073] Comparative Example 5
[0074] The preparation method steps used in this comparative example are the same as those in Example 1, except that no accelerating agent is contained. In this comparative example, the accelerating setting paste material comprises the following components in parts by weight: 150 parts of cement, 150 parts of fly ash, 70 parts of magnesium slag, 200 parts of coal gasification slag, 1200 parts of coal gangue, 0.8 parts of water reducing agent, and 260 parts of water.
[0075] The performance of the quick-setting paste material prepared in this comparative example was tested, and the results are shown in Table 5.
[0076] Final setting time / min Fluidity / (mm) Slump / (mm) 1d compressive strength / MPa 28d compressive strength / MPa Example 1 157 470 260 3.1 7.6 Example 2 152 486 271 2.8 7.1 Example 3 144 481 252 3.6 13.8 Comparative Example 1 162 482 265 2.6 6.5 Comparative Example 2 256 467 258 1.6 3.3 Comparative Example 3 152 410 239 2.7 6.5 Comparative Example 4 174 450 257 2.1 4.9 Comparative Example 5 532 442 247 0.4 2.7
[0077] Table 5. Test results of quick-setting paste material performance
[0078] It can be seen from Examples 1 to 3 that the preparation processes of Example 1, Example 2 and Example 3 are the same. In terms of material components, Example 2 reduces the dosage of the cementitious material component, and Example 3 increases the dosage of the cementitious material component. It can be seen from the performance test results that the dosage of the cementitious material can ensure the various properties of the material, which is specifically manifested in that a reduction in the dosage of the cementitious material component will increase the material setting time and reduce the material compressive strength; an increase in the dosage of the cementitious material component will shorten the material setting time and improve the material compressive strength.
[0079] It can be seen from Example 1 and Comparative Example 1 that after adding the accelerating agent, the setting time of the quick-setting paste materials prepared in Example 1 and Comparative Example 1 is within 3 hours, and both 1d and 28d have high strengths, but the compressive strength of Example 1 is significantly higher than that of Comparative Example 1. This is because: the components of Example 1 contain magnesium slag, and the carbon dioxide released by the reaction of sodium bicarbonate and aluminum sulfate carbonizes the magnesium slag to generate a large amount of carbonization products that fill between the hydration products of the cement, thereby making the prepared paste material structure more compact and improving the overall strength of the paste material. Figure 2 (b) It can be seen that the main elements of the obtained rod-shaped product are calcium, oxygen, sulfur, and aluminum (gold is caused by gold spraying when making electron microscope samples). It can be seen that the product is calcium sulfonate. In this fast-setting paste system, the early cement hydration product contains a large amount of calcium sulfonate.
[0080] Depend on Figure 2 (a) with Figure 3 By comparison, it can be seen that the internal structure of the product obtained in Example 1 is denser than that in Comparative Example 1. This is because the magnesium slag in Example 1 further reacts with the carbon dioxide released by sodium bicarbonate to generate a large amount of calcium carbonate, magnesium carbonate, silica gel and CSH gel, which then fill the structural gaps overlapped by the cement hydration product calcium sulfide, thereby making the structure denser.
[0081] It can be seen from Example 1 and Comparative Example 2 that the setting time of Example 1 is within 3 hours, while the setting time of Comparative Example 2 exceeds 4 hours, and the 1d and 28d strengths of Example 1 are significantly greater than those of Comparative Example 2. This is because the products generated by the reaction of aluminum sulfate and sodium bicarbonate are Al(OH)3 and CO2. The presence of Al(OH)3 can continuously promote the early hydration reaction of cement, while the presence of CO2 can induce the magnesium slag material to react and generate more reaction products. The synergistic effect of the two shortens the setting time of the paste material and improves the structural strength of the paste material.
[0082] Depend on Figure 2 and Figure 4 It can be seen that Figure 2 Contains a large amount of reaction products and has a dense structure. Figure 4 There are fewer reaction products and the structure is relatively loose, which shows that the addition of aluminum sulfate promotes the hydration and carbonization reactions of the material.
[0083] It can be seen from Example 1 and Comparative Example 3 that the fluidity and slump of Example 1 are better than those of Comparative Example 3, because the coal gasification slag particles contain more spherical particles (see Figure 1 ), the addition of coal gasification slag increases the spherical particle components inside the material, thereby reducing the friction between the components inside the material, improving the workability of the material, and increasing the fluidity of the material. It is also because the workability of the material is better that the components are dispersed more evenly. This is also the reason why the strength of Example 1 is greater than that of Comparative Example 3.
[0084] from Figure 5 It can be seen that the spherical particles of coal gasification slag are evenly distributed, which is the reason why the material has good fluidity.
[0085] It can be seen from Example 1 and Comparative Example 4 that the properties of Comparative Example 4 such as setting time, fluidity, and compressive strength have decreased to varying degrees. This is because the lack of sodium bicarbonate prevents the magnesium slag from undergoing a carbonization reaction, which results in less reaction products inside the material than in Example 1. Therefore, the setting time and compressive strength are not as good as those of Example 1. The fluidity of Comparative Example 4 is also not as good as that of Example 1 because of the presence of sodium bicarbonate, which releases carbon dioxide gas during the reaction. The presence of these gases improves the workability of the material to a certain extent, thereby increasing the fluidity of the material.
[0086] It can be seen from Comparative Example 5 that without adding an accelerator, the setting time of the prepared paste material exceeds 7 hours, and the 1d compressive strength and 28d compressive strength are low, which cannot meet the construction requirements. Therefore, the presence of the accelerator effectively guarantees the early performance of the material.
[0087] It can be seen from the above embodiments and comparative examples that the post-frame filling quick-setting paste material provided by the present invention has excellent fluidity and early strength. The addition of magnesium slag, coal gasification slag, sodium bicarbonate, and quick-setting agent in the system, as well as the control of the amount of cementitious material, ensure the various properties of the quick-setting paste material, so that the quick-setting paste material can control the cost while meeting the high fluidity and high early strength requirements. The excellent fluidity of the quick-setting paste material can meet the pumping requirements, the controllable setting time can meet the coal mining process requirements, and the higher early strength can strongly support the roof, thereby meeting the various performance requirements of the quick-setting paste material for filling mining at this stage.
[0088] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0089] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A method for preparing a quick-setting paste material, characterized in that: The method comprises the following steps: Step 1: Pour coal gangue and coal gasification slag into a stirring device, add water into the stirring device, mix and stir at a rate of 100 to 200 r / min for 1 to 3 minutes to obtain a mixed material A. Step 2: Add cement, fly ash, magnesium slag, water reducer and water to the mixed material A in sequence, mix and stir at a rate of 100 to 200 r / min for 3 to 5 minutes to obtain slurry B; Step 3, adding sodium bicarbonate and accelerating agent to slurry B, mixing and stirring at a rate of 100 to 200 r / min for 3 to 5 minutes, to obtain a quick-setting paste material; The quick-setting paste material comprises the following components in parts by weight: 100-200 parts of cement, 100-200 parts of fly ash, 50-100 parts of magnesium slag, 150-300 parts of coal gasification slag, 60-1200 parts of coal gangue, 8-16 parts of sodium bicarbonate, 0.2-1.0 parts of water reducing agent, 2-10 parts of quick-setting agent and 200-350 parts of water.
2. The method for preparing the quick-setting paste material according to claim 1, characterized in that: The accelerating setting agent is selected from one or more of sodium aluminate, aluminum sulfate, calcium sulfoaluminate and sodium sulfate.
3. The method for preparing the quick-setting paste material according to claim 1, characterized in that: The water reducer is selected from one or more of polycarboxylate water reducers and naphthalene water reducers.
4. The method for preparing the quick-setting paste material according to claim 1, characterized in that: At least 80% of the fly ash powder particle size is less than 45 μm; the particle size of the magnesium slag is less than 75 μm, the particle size of the coal gasification slag aggregate is 0.075 mm to 4.75 mm, and the particle size of the coal gangue aggregate is less than 20 mm.
5. The method for preparing the quick-setting paste material according to claim 1, characterized in that: The method comprises the following steps: Step 1: Pour coal gangue and coal gasification slag into a stirring device, add water into the stirring device, mix and stir at a rate of 100 r / min for 2 minutes to obtain a mixed material A. Step 2: Add cement, fly ash, magnesium slag, water reducer and water to the mixture A in sequence, mix and stir at a rate of 200 r / min for 3 minutes to obtain slurry B; Step 3, adding sodium bicarbonate and accelerating agent to slurry B, mixing and stirring at a rate of 200 r / min for 5 minutes, to obtain a quick-setting paste material; The quick-setting paste material comprises the following components by weight: 150 parts of cement, 150 parts of fly ash, 70 parts of magnesium slag, 200 parts of coal gasification slag, 1200 parts of coal gangue, 15 parts of sodium bicarbonate, 0.8 parts of water reducing agent, 6 parts of quick-setting agent and 260 parts of water.
6. A quick-setting paste material, which is prepared by the preparation method according to any one of claims 1 to 5.
7. The quick-setting paste material according to claim 6, characterized in that: The quick-setting paste material has a setting time of less than 3 hours, a 1-day compressive strength greater than 2 MPa, and a 28-day compressive strength greater than 5 MPa.
8. Use of the quick-setting paste material obtained by the preparation method according to any one of claims 1 to 5 for filling mining.
Citation Information
Cited By
Method for co-processing heavy salt water and sequestration carbon by underground filling
CN121322089A