Durable high-strength concrete pipe pile concrete and application

By using water-soluble silicone oil in PHC pipe pile concrete, the synergistic effect of composite binder and amine-based premature strength agent of nonionic water-enclosed isocyanate, the early strength and durability problems are solved, and high strength and low cracks are achieved concrete properties.

CN118930190APending Publication Date: 2024-11-12SHANDONG HUAWEI CONSTR TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411207168.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The early strength of existing PHC pipe pile concrete is difficult to reach C80 level after high-pressure steaming, and it is prone to problems such as excessive local cement ratio, enhanced brittleness, cracks and strength reduction, which affects its durability.

Method used

Using a composite binder of water-soluble silicone oil and nonionic water-enclosed isocyanate, bonded particles that can enhance the bonding of concrete by reacting isocyanate groups with water-soluble silicone oil, improve the toughness and durability of concrete, and utilize amines. The early strength agents of nitrates jointly promote hydration reactions and improve early strength.

Benefits of technology

It significantly improves the early strength and durability of pipe pile concrete, reduces cracks, prevents ion penetration, and meets the needs of early strength and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005019349900000041
    Figure BDA0005019349900000041
  • Figure BDA0005019349900000061
    Figure BDA0005019349900000061
Patent Text Reader

Abstract

The invention provides durable high-strength concrete tubular pile concrete and application, and the durable high-strength concrete tubular pile concrete is prepared from the following raw materials in parts by weight: 75-85 parts of Portland cement, 15-25 parts of admixture, 150-220 parts of fine aggregate, 260-400 parts of coarse aggregate, 1-1.5 parts of water reducing agent, 1.5-2 parts of early strength agent, 8-10 parts of binder and 23-30 parts of water, the binder is composed of nonionic water-based blocked isocyanate and water-soluble silicone oil according to the mass ratio of (0.6-0.8): 1. According to the invention, the water-soluble silicone oil and the non-ionic water-based blocked isocyanate are used as binders, the non-ionic water-based blocked isocyanate is de-blocked at a high temperature, and an isocyanate group reacts with hydroxyl on the water-soluble silicone oil to form bonding particles capable of enhancing the cohesiveness of concrete; the toughness of the pipe pile concrete can be improved, cracks are reduced, the strength is improved, ion permeation can be prevented, and the durability of the concrete is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pipe pile concrete, and in particular relates to a durable high-strength concrete pipe pile concrete and application thereof. Background Art

[0002] Prestressed high-strength concrete pipe piles (PHC pipe piles) are a type of prefabricated component. In order to avoid the premature appearance of cracks in reinforced concrete structures, high-strength steel bars and high-strength concrete are fully utilized to try to reduce the tensile stress of the components by applying external force before the concrete structure or components are subjected to the use load, and even concrete components in a compressive stress state. As a high-quality pile foundation material, PHC pipe piles have many advantages such as industrialized production, high unit bearing capacity, low cost, and fast construction. They are widely used in the foundation structures of bridges, tunnels, buildings, docks, ports, airports and other engineering construction.

[0003] As the application scope of PHC pipe piles is expanding, the durability problem is becoming more and more prominent, especially when pipe piles are used in coastal facilities such as ports and docks. The three main damages that reduce durability are corrosion damage of the pile body concrete, steel corrosion, and softening damage of the rock layer at the pile end. Because the pile body concrete is the core component of the pipe pile, the durability of the concrete has a decisive influence on the overall service life and performance of the pipe pile. Researchers have conducted a lot of research on the durability of the pipe pile concrete. For example, the durable PHC pipe pile concrete and PHC pipe pile disclosed in patent CN114804781B include the following components: 340-470 parts of cement, 30-50 parts of waterproof particles, 780-1300 parts of aggregates, 25-60 parts of mineral powder, 25-60 parts of fly ash, 3-5 parts of water reducer, and 68-94 parts of water; the waterproof particles include VAE emulsion, acrylic emulsion, and stone powder in a weight ratio of 1: (2-5): (15-22). The PHC pipe pile concrete and PHC pipe pile disclosed in patent CN114873985B include the following components by weight: 220-370 parts of cement, 1000-1400 parts of coarse aggregate, 3-11 parts of water reducer, 100-150 parts of water, 30-85 parts of fly ash, and 800-1000 parts of composite fine aggregate.

[0004] In order to improve the durability of pipe piles by combining the above technologies, researchers often use the filling and compacting effect of ultrafine mineral admixtures (such as silica sand powder, slag powder, fly ash, silica ash, zeolite powder, etc.) in prestressed concrete pipe piles to achieve dense accumulation between solid particles, thereby improving the density of concrete and improving durability. However, the early activity of mineral admixtures is low, resulting in the strength of PHC pipe pile concrete after high-pressure steam curing to be difficult to reach the C80 level that some companies have strict requirements for early strength. There may even be problems such as excessive local crystal-gel ratio, increased brittleness, cracks, and decreased strength. Therefore, it is necessary to develop a PHC pipe pile concrete with high early strength and good durability. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a durable high-strength concrete pipe pile concrete and its application. The pipe pile concrete includes a compound of water-soluble silicone oil and non-ionic water-based blocked isocyanate as a binder. The non-ionic water-based blocked isocyanate is deblocked at high temperature, and the isocyanate group reacts with the hydroxyl group on the water-soluble silicone oil to form bonding particles that can enhance the bonding of the concrete. It can not only improve the toughness of the pipe pile concrete, reduce cracks, and increase the strength, but also prevent ion penetration and improve the durability of the concrete.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] A durable high-strength concrete pipe pile concrete comprises the following raw materials in parts by weight: 75-85 parts of silicate cement, 15-25 parts of admixture, 150-220 parts of fine aggregate, 260-400 parts of coarse aggregate, 1-1.5 parts of water reducer, 1.5-2 parts of early strength agent, 8-10 parts of binder, and 23-30 parts of water, wherein the binder is composed of non-ionic water-based blocked isocyanate and water-soluble silicone oil in a mass ratio of 0.6-0.8:1.

[0008] The water-soluble silicone oil is a polysiloxane-polyalkoxy ether copolymer with a hydroxyl value of 40-45 mgKOH / g.

[0009] Water-soluble silicone oil is a polymer with active terminal hydroxyl side chains formed by hydrolysis of chlorosilane to form polysiloxane, which is then grafted and condensed with polyether. Because the end group of the polyether is hydroxyl, water-soluble silicone oil is a reactive silicone oil and is often used as a fabric finishing agent.

[0010] The nonionic water-based blocked isocyanate has a deblocking temperature of 90-110° C. and an NCO content of 4-5.5 wt %.

[0011] Water-based blocked isocyanates are commonly used as curing agents, crosslinking agents, and bridging agents for water-based adhesives. They can coexist stably with water-based resins (water-based polyurethanes, water-based acrylates, fluorine emulsions, silicone emulsions, etc.) for a long time at room temperature. The isocyanate (-NCO) group released by the curing agent during heat treatment reacts with hydroxyl, carboxyl, amino, and other groups on the water-based resin molecular chain to form a crosslinked structure. In the present invention, the nonionic water-based blocked isocyanate has good dispersibility in water at room temperature, has no adverse effects on the hydration and hardening process of fresh concrete, and releases isocyanate (-NCO) groups when encountering high temperatures of normal pressure steam curing. The isocyanate groups react with the active hydroxyl groups at the ends of the side chains of water-soluble silicone oils to form bonding particles that can enhance the bonding properties of concrete.

[0012] The early strength agent is selected from one or a combination of two or more of amine early strength agents and nitrate early strength agents.

[0013] Furthermore, the early strength agent is compounded by an amine early strength agent and a nitrate early strength agent in a mass ratio of 0.05-0.08:1; the amine early strength agent is selected from one or a combination of two or more of triethanolamine, triisopropanol, and diethanolamine; the nitrate early strength agent is selected from one or a combination of two or more of sodium nitrate, sodium nitrite, calcium nitrate, and calcium nitrite.

[0014] The admixture is selected from one or a combination of two or more of silica fume, fly ash, slag powder and metakaolin.

[0015] Furthermore, the admixture is formed by mixing slag powder, fly ash and silica fume in a mass ratio of 50-80:30-80:30-80.

[0016] Furthermore, the specific surface area of ​​the slag powder is 350-650m 2 / kg, 7-day activity index is not less than 85%, 28-day activity index is greater than 95%; the fly ash fineness is 20-25%, the water requirement is 80-100%, 7-day activity index is not less than 85%; the specific surface area of ​​the silica ash is greater than 18000m 2 / kg, and the activity index at 28 days was greater than 95%.

[0017] The strength grade of the silicate cement is 42.5-52.5.

[0018] The fine aggregate fineness modulus is 2.3-3.4.

[0019] The coarse aggregate is natural crushed stone with an average particle size of 5-25 mm. The coarse aggregate adopts continuous grading with a mass ratio of 5-10 mm sieve residue to 10-20 mm sieve residue of 1:3.5-4.0.

[0020] The water reducer is selected from one or a combination of polycarboxylic acid high-efficiency water reducer and naphthalene-based high-efficiency water reducer.

[0021] The present invention also provides a method for preparing the above durable high-strength concrete, comprising the following steps:

[0022] Add silicate cement, admixture, fine aggregate, coarse aggregate, admixture, water reducing agent, early strength agent, binder and water into a mixer and mix until uniform to obtain durable high-strength concrete.

[0023] The present invention also provides the use of the durable high-strength concrete in preparing PHC pipe piles.

[0024] Furthermore, the use comprises the following steps:

[0025] The durable high-strength concrete is injected into the pipe pile mold, the mold is closed, and the pipe pile mold after closing is subjected to prestressing tensioning treatment, the pipe pile mold is subjected to centrifugal treatment from low to high speed, steam curing, demoulding, and high-pressure steam curing to obtain a durable PHC pipe pile.

[0026] The steps of centrifugation from low to high speed are: centrifugation at a speed of 50-80 r / min for 1-3 min, increasing the speed to 100-150 r / min for 1-3 min, continuing to increase the speed to 200-400 r / min for 3-5 min, and finally increasing the speed to 400-600 r / min for 5-10 min.

[0027] The steam curing procedure includes four stages: static, heating, constant temperature and cooling. The static time is 0.5-3.5h, the heating rate in the heating stage is 20-30℃ / h, the temperature in the constant temperature stage is 80-100℃ and the time is 4-8h, and the cooling is natural cooling.

[0028] The high-pressure steam curing includes a temperature increase and pressure increase stage, a constant temperature and pressure stage, and a temperature decrease and pressure reduction stage. The temperature increase and pressure increase stage is to increase the pressure to 0.8-1MPa and the temperature to 160-180°C in 0.5-2.5h; the constant temperature and pressure stage is 4-6h; the temperature decrease and pressure reduction stage is a natural temperature decrease with a pressure reduction rate of 0.3-0.5MPa / h.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The present invention uses a compound of water-soluble silicone oil and non-ionic water-based blocked isocyanate as a binder, utilizes the non-ionic water-based blocked isocyanate to deblock at high temperature, and the isocyanate group reacts with the hydroxyl group on the water-soluble silicone oil to form bonding particles that can enhance the bonding of concrete. This can not only improve the toughness of pipe pile concrete, reduce cracks, and increase strength, but also prevent ion penetration and improve the durability of concrete.

[0031] The inventors found that the binder has a synergistic effect with the early strength agent composed of amine early strength agent and nitrate early strength agent in a mass ratio of 0.05-0.08:1, which significantly improves the early strength of pipe pile concrete. It is speculated that the binder and the early strength agent synergistically promote the hydration reaction. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with specific embodiments, but is not limited to the contents of the specification. Unless otherwise specified, the "parts" described in the embodiments of the present invention are all parts by weight. The reagents used are all commercially available reagents in the art.

[0033] JC2000 water-soluble silicone oil was purchased from Guangzhou Jucheng Zhaoye Silicone Raw Materials Co., Ltd., with a hydroxyl value of 41.4 mgKOH / g.

[0034] JC3000 water-soluble silicone oil was purchased from Guangzhou Jucheng Zhaoye Silicone Raw Materials Co., Ltd., with a hydroxyl value of 44.4 mgKOH / g.

[0035] Slag powder was purchased from Hebei Wenfeng Industrial Group Co., Ltd. with a specific surface area of ​​450m 2 / kg, 7-day activity index 88%, 28-day activity index 101%.

[0036] The fly ash was purchased from Hebei Wenfeng Industrial Group Co., Ltd. The fly ash fineness was 23.6%, the water requirement ratio was 98%, and the 7-day activity index was 95%.

[0037] Silica fume was purchased from Hebei Wenfeng Industrial Group Co., Ltd. The specific surface area of ​​silica fume is 18600m 2 / kg, activity index at 28 days was 98%.

[0038] Fine aggregate was purchased from Zhuzhou Aggregate New Materials Co., Ltd., with a 4.75 mm sieve residue of 3%, a 2.36 mm sieve residue of 12%, a 1.18 mm sieve residue of 23%, a 0.6 mm sieve residue of 46%, a 0.3 mm sieve residue of 78%, and a 0.5 mm sieve residue of 99%.

[0039] Coarse aggregate was purchased from Zhuzhou Aggregate New Materials Co., Ltd. The screening results of 5-10mm and 10-20mm crushed stone are as follows:

[0040]

[0041] The high-efficiency water reducing agent was purchased from BASF, with the brand name Melflux 4930F.

[0042] Non-ionic water-based blocked isocyanate was purchased from Changzhou Houding Chemical Co., Ltd. with a brand name of HD-8035, a blocking temperature of 107° C., and an NCO content of 5.5 wt %.

[0043] Example 1

[0044] 1) 75 parts by mass of P.Ⅱ42.5 silicate cement, 25 parts by mass of an admixture prepared by mixing slag powder, fly ash and silica fume in a mass ratio of 50:80:80, 165 parts by mass of fine aggregate, 285 parts by mass of coarse aggregate, 1.5 parts by mass of high-efficiency water reducing agent Melflux 4930F, 2.0 parts by mass of an early strength agent prepared by compounding triethanolamine and sodium nitrate in a mass ratio of 0.08:1, 10 parts by mass of a binder prepared by mixing non-ionic water-based blocked isocyanate HD-8035 and water-soluble hydroxy silicone oil JC2000 in a mass ratio of 0.6:1, and 27 parts by mass of water were added to a mixer and mixed until uniform to obtain durable high-strength concrete;

[0045] 2) Inject durable high-strength concrete into the pipe pile mold, close the mold, and perform prestressing tensioning treatment on the pipe pile mold after closing the mold, centrifugal treatment, steam curing, demoulding, and high-pressure steam curing on the pipe pile mold to obtain a durable PHC pipe pile.

[0046] Centrifugation: low speed stage at 60r / min for 2min, low-medium speed stage at 115r / min for 2min, medium speed stage at 290r / min for 4min, and high speed stage at 480r / min for 7min.

[0047] Steam curing: stop for 0.5h, heat up to 100℃ at a rate of 25℃ / h, keep constant at 100℃ for 5h, and naturally cool down to room temperature;

[0048] High-pressure steam curing: During the temperature and pressure increase stage, the pressure is increased to 0.88MPa for 2h, the temperature is increased to 180℃, and during the constant temperature and pressure stage, 180℃ and 0.88MPa are maintained at constant temperature and pressure for 5h. During the temperature and pressure reduction stage, natural cooling is adopted, and the reduction rate is 0.3MPa / h.

[0049] Example 2

[0050] The rest is the same as Example 1, except that JC2000 is replaced by JC3000 of equal mass.

[0051] Example 3

[0052] The rest is the same as Example 1, except that the binder is composed of non-ionic water-based blocked isocyanate HD-8035 and water-soluble hydroxy silicone oil JC2000 in a mass ratio of 0.8:1.

[0053] Example 4

[0054] The rest is the same as Example 1, except that the amount of the binder is 8 parts by mass.

[0055] Example 5

[0056] The rest is the same as Example 1, except that the amount of the binder is 12 parts by mass.

[0057] Example 6

[0058] The rest is the same as Example 1, except that the amount of the binder is 6 parts by mass.

[0059] Example 7

[0060] The rest is the same as Example 1, except that, in step 1), 85 parts by mass of P.Ⅱ42.5 silicate cement, 15 parts by mass of an admixture prepared by mixing slag powder, fly ash, and silica ash in a mass ratio of 80:30:80, 165 parts by mass of fine aggregate, 285 parts by mass of coarse aggregate, 1.0 parts by mass of a high-efficiency water reducer Melflux 4930F, 1.5 parts by mass of an early strength agent prepared by compounding triethanolamine and sodium nitrate in a mass ratio of 0.05:1, 8 parts by mass of a binder composed of non-ionic water-based blocked isocyanate HD-8035 and water-soluble hydroxy silicone oil JC2000 in a mass ratio of 0.8:1, and 27 parts by mass of water are added to a mixer and mixed until uniform to obtain durable high-strength concrete.

[0061] Example 8

[0062] The rest is the same as Example 1, except that the early strength agent is all triethanolamine.

[0063] Example 9

[0064] The rest is the same as Example 1, except that the early strength agent is all sodium nitrate.

[0065] Comparative Example 1

[0066] The rest is the same as Example 1, except that the water-soluble silicone oil is replaced by an equal mass of Bayer polyether polyol Multranol 9159 (hydroxyl value: 46.5 mgKOH / g).

[0067] Comparative Example 2

[0068] The rest is the same as Example 1, except that the nonionic water-based blocked isocyanate HD-8035 is not added.

[0069] Comparative Example 3

[0070] The rest is the same as Example 1, except that no binder is added.

[0071] The pipe pile concrete prepared in the above embodiments and comparative examples was subjected to the following performance tests:

[0072] Slump: Tested in accordance with standard GB / T 8076-2008 concrete admixtures.

[0073] Compressive strength: The compressive strength is tested in accordance with the standard GB / T 50081-2002 Test method for mechanical properties of ordinary concrete.

[0074] Resistance to chloride ion penetration: The electric flux method in the GB / T 50082-2009 standard for test methods for long-term performance and durability of ordinary concrete. The smaller the electric flux value, the better the resistance to chloride ion penetration.

[0075] Table 1 Performance test results

[0076]

[0077] It can be seen from Table 1 that the pipe pile concrete prepared by the binder composed of water-soluble silicone oil and non-ionic water-based blocked isocyanate has good early strength, can also prevent ion penetration and improve the durability of concrete.

[0078] It can be seen from the compressive strength of the embodiments and the comparative examples that the binder has the effect of synergizing with the early strength agent composed of an amine early strength agent and a nitrate early strength agent in a mass ratio of 0.05-0.08:1 to significantly improve the early strength of the pipe pile concrete. It is speculated that the binder and the early strength agent synergistically promote the hydration reaction.

[0079] The above detailed description is a specific description of one feasible embodiment of the present invention. The embodiment is not intended to limit the patent scope of the present invention. Any equivalent implementation or modification that does not deviate from the present invention should be included in the scope of the technical solution of the present invention.

Claims

1. A durable high-strength concrete pipe pile concrete, characterized in that: The invention comprises the following raw materials in parts by weight: 75-85 parts of silicate cement, 15-25 parts of admixture, 150-220 parts of fine aggregate, 260-400 parts of coarse aggregate, 1-1.5 parts of water reducer, 1.5-2 parts of early strength agent, 8-10 parts of binder and 23-30 parts of water, wherein the binder is composed of non-ionic water-based blocked isocyanate and water-soluble silicone oil in a mass ratio of 0.6-0.8:

1.

2. The durable high-strength concrete pipe pile concrete according to claim 1, characterized in that: The water-soluble silicone oil is a polysiloxane-polyalkoxy ether copolymer with a hydroxyl value of 40-45 mgKOH / g.

3. The durable high-strength concrete pipe pile concrete according to claim 1, characterized in that: The nonionic water-based blocked isocyanate has a deblocking temperature of 90-110° C. and an NCO content of 4-5.5 wt %.

4. The durable high-strength concrete pipe pile concrete according to claim 1, characterized in that: The early strength agent is selected from one or a combination of two or more of amine early strength agents and nitrate early strength agents; preferably, the amine early strength agent is selected from one or a combination of two or more of triethanolamine, triisopropanolamine, and diethanolamine; the nitrate early strength agent is selected from one or a combination of two or more of sodium nitrate, sodium nitrite, calcium nitrate, and calcium nitrite.

5. The durable high-strength concrete pipe pile concrete according to claim 4, characterized in that: The early strength agent is prepared by compounding an amine early strength agent and a nitrate early strength agent at a mass ratio of 0.05-0.08:

1.

6. The durable high-strength concrete pipe pile concrete according to claim 1, characterized in that: The admixture is selected from one or a combination of two or more of silica fume, fly ash, slag powder and metakaolin.

7. The durable high-strength concrete pipe pile concrete according to claim 6, characterized in that: The admixture is prepared by mixing slag powder, fly ash and silica ash in a mass ratio of 50-80:30-80:30-80.

8. The durable high-strength concrete pipe pile concrete according to claim 6, characterized in that: The specific surface area of ​​the slag powder is 350-650m 2 / kg, 7-day activity index is not less than 85%, 28-day activity index is greater than 95%; the fly ash fineness is 20-25%, the water requirement is 80-100%, 7-day activity index is not less than 85%; the specific surface area of ​​the silica ash is greater than 18000m 2 / kg, and the activity index at 28 days was greater than 95%.

9. The method for preparing the durable high-strength concrete according to any one of claims 1 to 8, comprising the following steps: Add silicate cement, admixture, fine aggregate, coarse aggregate, admixture, water reducing agent, early strength agent, binder and water into a mixer and mix until uniform to obtain durable high-strength concrete.

10. Use of the durable high-strength concrete according to any one of claims 1 to 8 in preparing PHC piles; Furthermore, the use comprises the following steps: The durable high-strength concrete is injected into the pipe pile mold, the mold is closed, and the pipe pile mold after the mold is closed is subjected to prestressing tensioning treatment, the pipe pile mold is subjected to centrifugal treatment from low to high speed, steam curing, demoulding, and high-pressure steam curing to obtain a durable PHC pipe pile; Preferably, the steps of centrifugation from low to high speed are centrifugation at a speed of 50-80 r / min for 1-3 min, Increase the speed to 100-150r / min and centrifuge for 1-3 minutes, then continue to increase the speed to 200-400r / min and centrifuge for 3-5 minutes. Finally, increase the speed to 400-600r / min and centrifuge for 5-10 minutes.