Barium-doped indium tin zinc oxide target material and preparation method thereof
By adding Ba elements into ITZO targets and using wet grinding and spray granulation technology, barium-doped indium tin oxide targets was prepared, which solved the problems of many target defects and high resistance, and improved the film mobility and light transmittance enhances the stability of the film.
Patent Information
- Application Number
- CN202411284891.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-12
AI Technical Summary
There are many defects and high resistance during the preparation process of existing ITZO targets, which affect the performance and stability of the film.
By adding Ba elements into the ITZO target, wet grinding and spray granulation technology are used to prepare barium-doped indium tin zinc targets to reduce defects in the target and reduce resistance. Specific steps include material extraction according to a specific ratio, wet grinding, spray granulation, degreasing heat treatment and sintering heat treatment.
The combination of metal elements and oxygen elements in the target material is improved, the target material defects are reduced, the resistance is reduced, the film mobility and light transmittance are improved, and the film stability is enhanced.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of target material preparation, and more specifically, relates to a barium-doped indium tin zinc oxide target material and a preparation method thereof. Background Art
[0002] Oxide semiconductor films have excellent properties of high electron mobility, high transmittance and low growth temperature. They have partially replaced traditional silicon-based thin film transistors and become the next generation display technology driver devices.
[0003] Among the known oxide semiconductor films, amorphous ITZO film is one of the most excellent materials. Today, ITZO films are mainly prepared by magnetron sputtering, which requires the use of high-performance ITZO targets. The relative density, microstructure, electrical properties and other properties of ITZO targets are closely related to the performance of sputtered films.
[0004] Therefore, in order to obtain high-performance ITZO thin films, it is necessary to develop a high-quality ITZO target. Summary of the invention
[0005] In view of the above problems existing in the prior art, one of the objects of the present invention is to provide a method for preparing a barium-doped indium tin zinc oxide target, by adding Ba element into the ITZO target, thereby reducing the generation of defects in the target and lowering the resistance of the target.
[0006] A second object of the present invention is to provide a barium-doped indium tin zinc oxide target.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is: A method for preparing a barium-doped indium tin zinc oxide target comprises the following steps: (1) Weigh indium oxide powder, tin oxide powder, zinc oxide powder, and barium oxide powder in a mass ratio of 84-92.5:5-10:0.5-2:2-4; (2) Pour zinc oxide powder, tin oxide powder and a first dispersant into a container containing pure water, disperse them uniformly, and then perform wet grinding to obtain slurry 1; (3) adding barium oxide powder and a second dispersant to slurry 1, dispersing them uniformly, and then wet grinding them to obtain slurry 2; (4) adding indium oxide powder and a third dispersant to slurry 2, dispersing them uniformly, and then wet grinding them to obtain slurry 3; (5) adding a binder to slurry 3, dispersing the slurry evenly, and then wet grinding the slurry to obtain slurry 4; (6) using slurry 4 as a raw material to perform spray granulation to obtain barium-doped indium tin zinc oxide powder; (7) using barium-doped indium tin zinc oxide powder as a raw material for pressing and molding to obtain a barium-doped indium tin zinc oxide target blank; (8) The barium-doped indium tin zinc oxide target blank is subjected to degreasing heat treatment and sintering heat treatment in sequence to obtain a barium-doped indium tin zinc oxide target material.
[0008] Preferably, the purity of tin oxide is 4N, the purity of tin oxide is 4N, the purity of zinc oxide is 4N, and the purity of barium oxide powder is 4N.
[0009] Preferably, the first dispersant, the second dispersant or the third dispersant is at least two of polyvinyl pyrrolidone (PVP), sodium dodecylbenzene sulfonate (SDBS) and sodium hexadecylbenzene sulfonate.
[0010] Preferably, the binder is at least two of a mixture of polyvinyl alcohol (PVA) and polyethylene glycol (PEG), polyvinyl alcohol (PVA), and polyvinyl butyral (PVB).
[0011] Preferably, the first dispersant accounts for 1-5% of the total mass of the added tin oxide powder and zinc oxide powder, pure water and the first dispersant.
[0012] Preferably, the second dispersant accounts for 1-15% of the total mass of the added barium oxide powder and the second dispersant.
[0013] Preferably, the third dispersant accounts for 1-15% of the total mass of the added indium oxide powder and the third dispersant.
[0014] Preferably, the binder accounts for 5-15% of the total mass of all added tin oxide powder, indium oxide powder, barium oxide powder, zinc oxide powder, the first dispersant, the second dispersant, the third dispersant and the binder.
[0015] Preferably, the solid content of the slurry 1 is 60-70%.
[0016] Preferably, the solid content of the slurry 2 is 60-70%.
[0017] Preferably, the solid content of the slurry three is 60-70%.
[0018] Preferably, the solid content of the slurry 24 is 60-70%.
[0019] Further preferably, the solid content of slurry one, slurry two, slurry three and slurry four is 65%.
[0020] Preferably, in step (6), spray granulation is carried out using a spray drying tower.
[0021] Further preferably, during the spray granulation process: the outlet air temperature of the spray drying tower is 70-85° C., and the atomizer frequency is 110-130 Hz.
[0022] Furthermore, the powder obtained after spray granulation is homogenized and sieved to obtain a powder with uniform particle size distribution.
[0023] Preferably, in step (7), compression molding is performed by cold isostatic pressing followed by molding.
[0024] Preferably, in step (8), the degreasing heat treatment is: in an air atmosphere, heating to 400°C-600°C at a heating rate of 0.1-0.5°C / min, and keeping the temperature for 6-12 hours.
[0025] Preferably, in step (8), the sintering heat treatment is: in an oxygen atmosphere, heating to 1400°C~1600°C at a heating rate of 0.5~1.5°C / min, and keeping the temperature for 8~12h.
[0026] Further preferably, during the sintering heat treatment process, the oxygen flow rate is 20-50 L / min.
[0027] The invention also discloses a barium-doped indium tin zinc oxide target material prepared by the method for preparing the barium-doped indium tin zinc oxide target material.
[0028] Compared with the prior art, the present invention has the following beneficial effects: During the preparation process of the barium-doped indium tin zinc oxide target material of the present application, the introduction of the barium element strengthens the combination of the metal element and the oxygen element in the unit cell, reduces the generation of defects in the target material, and reduces the resistance of the target material.
[0029] After sputtering and forming a film using the target material prepared in the present application, the mobility and transmittance of the obtained film are improved, and the reduction of defects also improves the stability of the film. DETAILED DESCRIPTION
[0030] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.
[0031] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0032] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0033] Example 1 (1) Weigh indium oxide, tin oxide, zinc oxide, and barium oxide powders in a mass ratio of 86:10:2:2 and set aside.
[0034] (2) Add a certain amount of pure water into the slurry barrel, and add the tin oxide and zinc oxide powders weighed in step (1) and PVP into the slurry barrel in sequence for pre-dispersion. The dispersion time is 30 min and the dispersion speed is 100 rpm, wherein PVP accounts for 4% of the total mass of the added tin oxide powder, zinc oxide powder, pure water and PVP.
[0035] The obtained slurry was pumped into a sand mill for grinding with a pneumatic diaphragm pump. The grinding time was 6 h and the grinding speed was 1500 r / min to obtain slurry 1 with a solid content of 65%.
[0036] (3) Add barium oxide powder and PVP to slurry 1 for dispersion. The dispersion time is 30 min and the dispersion speed is 100 rpm. The PVP accounts for 4% of the total mass of the added barium oxide powder and PVP.
[0037] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 rpm to obtain slurry 2 with a solid content of 65%.
[0038] (4) Add indium oxide powder and PVP into the slurry for dispersion, the dispersion time is 30 minutes, and the dispersion speed is 100 rpm. PVP accounts for 4% of the total mass of the added indium oxide powder and PVP.
[0039] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 12 h and the grinding speed was 1500 rpm to obtain slurry three with a solid content of 65%.
[0040] (5) PVA was added to slurry 3 and pre-dispersed. The pre-dispersion time was 30 min and the dispersion speed was 100 rpm. The binder accounted for 10% of the total mass of all added tin oxide powder, indium oxide powder, barium oxide powder, zinc oxide powder, the first dispersant, the second dispersant, the third dispersant and the binder.
[0041] The slurry was then pumped into a sand mill using a pneumatic diaphragm pump for grinding. The grinding time was 2 h and the grinding speed was 1500 rpm to obtain slurry 4 with a solid content of 65%.
[0042] (6) The slurry 4 is fed into a spray drying tower for spray granulation, and then mixed and sieved to obtain an indium tin zinc oxide mixed powder. The air outlet temperature is 75°C and the atomizer frequency is 120 Hz.
[0043] (7) The mixed powder obtained in step (6) is molded and then cold isostatically pressed to obtain a barium-doped indium tin zinc oxide target blank. Conventional cold isostatic pressing molding processes and parameters in the art can be used.
[0044] (8) The target blank obtained in step (7) is placed in a sintering furnace for degreasing heat treatment. In an air atmosphere, the temperature is controlled at 500°C at a heating rate of 0.5 / min, and then cooled to room temperature after a holding time of 8 hours to remove additives and other organic matter in the target blank.
[0045] (9) The target blank obtained in step (9) is placed in a sintering furnace for sintering in an oxygen atmosphere at a heating rate of 1°C / min. The temperature is raised to 1500°C and then kept at this temperature for 10 hours to obtain a barium-doped indium tin zinc oxide target.
[0046] Example 2 (1) Weigh indium oxide, tin oxide, zinc oxide, and barium oxide powders in a mass ratio of 86:10:2:2 and set aside.
[0047] (2) Add a certain amount of pure water into the slurry barrel, and add the tin oxide and zinc oxide powders weighed in step (1) and PVP into the slurry barrel in sequence for pre-dispersion. The dispersion time is 30 min and the dispersion speed is 100 rpm, wherein PVP accounts for 4% of the total mass of the added tin oxide powder, zinc oxide powder, pure water and PVP.
[0048] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 r / min to obtain slurry 1 with a solid content of 68%.
[0049] (3) Add barium oxide powder and PVP to slurry 1 for dispersion, the dispersion time is 30 minutes, and the dispersion speed is 100 rpm. PVP accounts for 4% of the total mass of the added barium oxide powder and PVP.
[0050] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 rpm to obtain slurry 2 with a solid content of 68%.
[0051] (4) Add indium oxide powder and PVP to slurry 2 for dispersion, with a dispersion time of 30 min and a dispersion speed of 100 rpm. PVP accounts for 4% of the total mass of the added indium oxide powder and PVP.
[0052] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 12 h and the grinding speed was 1500 rpm to obtain slurry three with a solid content of 68%.
[0053] (5) PVA was added to slurry 3 and pre-dispersed. The pre-dispersion time was 30 min and the dispersion speed was 100 rpm. The binder accounted for 10% of the mass of all the added substances.
[0054] The slurry was pumped into a sand mill with a pneumatic diaphragm pump for grinding. The grinding time was 2 h and the grinding speed was 1500 rpm to obtain slurry 4 with a solid content of 68%.
[0055] (6) The slurry 4 is fed into a spray drying tower for spray granulation, and then mixed and sieved to obtain an indium tin zinc oxide mixed powder. The air outlet temperature is 75°C and the atomizer frequency is 120 Hz.
[0056] (7) The mixed powder obtained in step (6) is molded by molding and then cold isostatic pressing to obtain a barium-doped indium tin zinc oxide target blank.
[0057] (8) The target blank obtained in step (7) is placed in a sintering furnace for degreasing heat treatment. In an air atmosphere, the temperature is controlled at 500°C at a heating rate of 0.5 / min, and then cooled to room temperature after a holding time of 8 hours to remove additives and other organic matter in the target blank.
[0058] (9) The target blank obtained in step (8) is placed in a sintering furnace for sintering in an oxygen atmosphere at a heating rate of 1°C / min. The temperature is raised to 1400°C and then kept at this temperature for 10 hours to obtain a barium-doped indium tin zinc oxide target.
[0059] Example 3 (1) Weigh indium oxide, tin oxide, zinc oxide, and barium oxide powders in a mass ratio of 85:10:2:3 and set aside.
[0060] (2) Add a certain amount of pure water into the slurry barrel, and add the tin oxide and zinc oxide powders weighed in step (1) and PVP into the slurry barrel in sequence for pre-dispersion. The dispersion time is 30 min and the dispersion speed is 100 rpm, wherein PVP accounts for 4% of the total mass of the added tin oxide powder, zinc oxide powder, pure water and PVP.
[0061] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 r / min to obtain slurry 1 with a solid content of 65%.
[0062] (3) Add barium oxide powder and PVP to slurry 1 for dispersion, the dispersion time is 30 minutes, and the dispersion speed is 100 rpm. PVP accounts for 4% of the total mass of the added barium oxide powder and PVP.
[0063] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 rpm to obtain slurry 2 with a solid content of 65%.
[0064] (4) Add indium oxide powder and PVP into the slurry for dispersion, the dispersion time is 30 minutes, and the dispersion speed is 100 rpm. PVP accounts for 4% of the total mass of the added indium oxide powder and PVP.
[0065] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 12 h and the grinding speed was 1500 rpm to obtain slurry three with a solid content of 65%.
[0066] (5) PVA was added to slurry 3 and pre-dispersed. The pre-dispersion time was 30 min and the dispersion speed was 100 rpm. The binder accounted for 10% of the mass of all the added substances.
[0067] The slurry was then pumped into a sand mill using a pneumatic diaphragm pump for grinding. The grinding time was 2 h and the grinding speed was 1500 rpm to obtain slurry 4 with a solid content of 65%.
[0068] (6) The slurry 4 is fed into a spray drying tower for spray granulation, and then mixed and sieved to obtain an indium tin zinc oxide mixed powder. The air outlet temperature is 75°C and the atomizer frequency is 120 Hz.
[0069] (7) The mixed powder obtained in step (6) is molded by molding and then cold isostatic pressing to obtain a barium-doped indium tin zinc oxide target blank.
[0070] (8) The target blank obtained in step (7) is placed in a sintering furnace for degreasing heat treatment. In an air atmosphere, the temperature is controlled at 500°C at a heating rate of 0.5 / min, and then cooled to room temperature after a holding time of 8 hours to remove additives and other organic matter in the target blank.
[0071] (9) The target blank obtained in step (8) is placed in a sintering furnace for sintering in an oxygen atmosphere at a heating rate of 1°C / min. The temperature is raised to 1500°C and then kept at this temperature for 10 hours to obtain a barium-doped indium tin zinc oxide target.
[0072] Example 4 (1) Weigh indium oxide, tin oxide, zinc oxide, and barium oxide powders in a mass ratio of 85:10:2:3 and set aside.
[0073] (2) Add a certain amount of pure water into the slurry barrel, and add the tin oxide and zinc oxide powders weighed in step (1) and PVP into the slurry barrel in sequence for pre-dispersion. The dispersion time is 30 min and the dispersion speed is 100 rpm, wherein PVP accounts for 4% of the total mass of the added tin oxide powder, zinc oxide powder, pure water and PVP.
[0074] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 r / min to obtain slurry 1 with a solid content of 60%.
[0075] (3) Add barium oxide powder and PVP to slurry 1 for dispersion, the dispersion time is 30 minutes, and the dispersion speed is 100 rpm. PVP accounts for 4% of the total mass of the added barium oxide powder and PVP.
[0076] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 rpm to obtain slurry 2 with a solid content of 60%.
[0077] (4) Add indium oxide powder and PVP to slurry 2 for dispersion, with a dispersion time of 30 min and a dispersion speed of 100 rpm. PVP accounts for 4% of the total mass of the added indium oxide powder and PVP.
[0078] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 12 h and the grinding speed was 1500 rpm to obtain slurry three with a solid content of 60%.
[0079] (5) PVA was added to slurry 3 and pre-dispersed. The pre-dispersion time was 30 min and the dispersion speed was 100 rpm. The binder accounted for 10% of the mass of all the added substances.
[0080] The slurry was then pumped into a sand mill using a pneumatic diaphragm pump for grinding. The grinding time was 2 h and the grinding speed was 1500 rpm to obtain slurry 4 with a solid content of 60%.
[0081] (6) The slurry 4 is fed into a spray drying tower for spray granulation, and then mixed and sieved to obtain an indium tin zinc oxide mixed powder. The air outlet temperature is 75°C and the atomizer frequency is 120 Hz.
[0082] (7) The mixed powder obtained in step (6) is molded by molding and then cold isostatic pressing to obtain a barium-doped indium tin zinc oxide target blank.
[0083] (8) The target blank obtained in step (7) is placed in a sintering furnace for degreasing heat treatment. In an air atmosphere, the temperature is controlled at 500°C at a heating rate of 0.5 / min, and then cooled to room temperature after a holding time of 8 hours to remove additives and other organic matter in the target blank.
[0084] (9) The target blank obtained in step (8) is placed in a sintering furnace for sintering in an oxygen atmosphere at a heating rate of 1°C / min. The temperature is raised to 1400°C and then kept at this temperature for 10 hours to obtain a barium-doped indium tin zinc oxide target.
[0085] Example 5 (1) Weigh indium oxide, tin oxide, zinc oxide, and barium oxide powders in a mass ratio of 84:10:2:4 and set aside.
[0086] (2) Add a certain amount of pure water into the slurry barrel, and add the tin oxide and zinc oxide powders weighed in step (1) and PVP into the slurry barrel in sequence for pre-dispersion. The dispersion time is 30 min and the dispersion speed is 100 rpm, wherein PVP accounts for 4% of the total mass of the added tin oxide powder, zinc oxide powder, pure water and PVP.
[0087] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 r / min to obtain slurry 1 with a solid content of 70%.
[0088] (3) Add barium oxide powder and PVP to slurry 1 for dispersion, the dispersion time is 30 minutes, and the dispersion speed is 100 rpm. PVP accounts for 4% of the total mass of the added barium oxide powder and PVP.
[0089] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 h and the grinding speed was 1500 rpm to obtain slurry 2 with a solid content of 70%.
[0090] (4) Add indium oxide powder and PVP to slurry 2 for dispersion, with a dispersion time of 30 min and a dispersion speed of 100 rpm. PVP accounts for 4% of the total mass of the added indium oxide powder and PVP.
[0091] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 12 h and the grinding speed was 1500 rpm to obtain slurry three with a solid content of 70%.
[0092] (5) PVA was added to slurry 3 and pre-dispersed. The pre-dispersion time was 30 min and the dispersion speed was 100 rpm. The binder accounted for 10% of the mass of all the added substances.
[0093] The slurry was then pumped into a sand mill using a pneumatic diaphragm pump for grinding. The grinding time was 2 h and the grinding speed was 1500 rpm to obtain slurry 4 with a solid content of 70%.
[0094] (6) The slurry 4 is fed into a spray drying tower for spray granulation, and then mixed and sieved to obtain an indium tin zinc oxide mixed powder. The air outlet temperature is 75°C and the atomizer frequency is 120 Hz.
[0095] (7) The mixed powder obtained in step (6) is molded by molding and then cold isostatic pressing to obtain a barium-doped indium tin zinc oxide target blank.
[0096] (8) The target blank obtained in step (7) is placed in a sintering furnace for degreasing heat treatment. In an air atmosphere, the temperature is controlled at 500°C at a heating rate of 0.5 / min, and then cooled to room temperature after a holding time of 8 hours to remove additives and other organic matter in the target blank.
[0097] (9) The target blank obtained in step (8) is placed in a sintering furnace for sintering in an oxygen atmosphere at a heating rate of 1°C / min. The temperature is raised to 1500°C and then kept at this temperature for 10 hours to obtain a barium-doped indium tin zinc oxide target.
[0098] Comparative Example 1 (1) Weigh indium oxide, tin oxide, zinc oxide, and barium oxide powders in a mass ratio of 85:10:2:3 and set aside.
[0099] (2) Add a certain amount of pure water into the slurry barrel, and add the tin oxide and zinc oxide powders weighed in step (1) and PVP into the slurry barrel in sequence for pre-dispersion. The dispersion time is 30 min and the dispersion speed is 100 rpm, wherein PVP accounts for 4% of the total mass of the added tin oxide powder, zinc oxide powder, pure water and PVP.
[0100] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 r / min to obtain slurry 1 with a solid content of 65%.
[0101] (3) Add barium oxide powder and PVP to slurry 1 for dispersion, the dispersion time is 30 minutes, and the dispersion speed is 100 rpm. PVP accounts for 4% of the total mass of the added barium oxide powder and PVP.
[0102] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 rpm to obtain slurry 2 with a solid content of 65%.
[0103] (4) Add indium oxide powder and PVP to slurry 2 for dispersion, with a dispersion time of 30 min and a dispersion speed of 100 rpm. PVP accounts for 4% of the total mass of the added indium oxide powder and PVP.
[0104] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 12 h and the grinding speed was 1500 rpm to obtain slurry three with a solid content of 65%.
[0105] (5) PVA was added to slurry 3 and pre-dispersed. The pre-dispersion time was 30 min and the dispersion speed was 100 rpm. The binder accounted for 10% of the mass of all the added substances.
[0106] The slurry was then pumped into a sand mill using a pneumatic diaphragm pump for grinding. The grinding time was 2 h and the grinding speed was 1500 rpm to obtain slurry 4 with a solid content of 65%.
[0107] (6) The slurry 4 is fed into a spray drying tower for spray granulation, and then mixed and sieved to obtain an indium tin zinc oxide mixed powder. The air outlet temperature is 75°C and the atomizer frequency is 120 Hz.
[0108] (7) The mixed powder obtained in step (6) is molded by molding and then cold isostatic pressing to obtain a barium-doped indium tin zinc oxide target blank.
[0109] (8) The target blank obtained in step (7) is placed in a sintering furnace for degreasing heat treatment. In an air atmosphere, the temperature is controlled at 500°C at a heating rate of 0.5 / min, and then cooled to room temperature after a holding time of 8 hours to remove additives and other organic matter in the target blank.
[0110] (9) The target blank obtained in step (8) is placed in a sintering furnace for sintering in an oxygen atmosphere at a heating rate of 1°C / min. The temperature is raised to 1200°C and then kept at this temperature for 10 hours to obtain a barium-doped indium tin zinc oxide target.
[0111] Comparative Example 2 (1) Weigh indium oxide, tin oxide, zinc oxide, and barium oxide powders in a mass ratio of 85:10:2:3 and set aside.
[0112] (2) Add a certain amount of pure water into the slurry barrel, and add the tin oxide and zinc oxide powders weighed in step (1) and PVP into the slurry barrel in sequence for pre-dispersion. The dispersion time is 30 min and the dispersion speed is 100 rpm, wherein PVP accounts for 4% of the total mass of the added tin oxide powder, zinc oxide powder, pure water and PVP.
[0113] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 r / min to obtain slurry 1 with a solid content of 65%.
[0114] (3) Add barium oxide powder and PVP to slurry 1 for dispersion, the dispersion time is 30 minutes, and the dispersion speed is 100 rpm. PVP accounts for 4% of the total mass of the added barium oxide powder and PVP.
[0115] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 rpm to obtain slurry 2 with a solid content of 65%.
[0116] (4) Add indium oxide powder and PVP to slurry 2 for dispersion, with a dispersion time of 30 min and a dispersion speed of 100 rpm. PVP accounts for 4% of the total mass of the added indium oxide powder and PVP.
[0117] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 12 h and the grinding speed was 1500 rpm to obtain slurry three with a solid content of 65%.
[0118] (5) PVA was added to slurry 3 and pre-dispersed. The pre-dispersion time was 30 min and the dispersion speed was 100 rpm. The binder accounted for 10% of the mass of all the added substances.
[0119] The slurry was then pumped into a sand mill using a pneumatic diaphragm pump for grinding. The grinding time was 2 h and the grinding speed was 1500 rpm to obtain slurry 4 with a solid content of 65%.
[0120] (6) The slurry 4 is fed into a spray drying tower for spray granulation, and then mixed and sieved to obtain an indium tin zinc oxide mixed powder. The air outlet temperature is 75°C and the atomizer frequency is 120 Hz.
[0121] (7) The mixed powder obtained in step (6) is molded by molding and then cold isostatic pressing to obtain a barium-doped indium tin zinc oxide target blank.
[0122] (8) The target blank obtained in step (7) is placed in a sintering furnace for degreasing heat treatment. In an air atmosphere, the temperature is controlled at 500°C at a heating rate of 0.5 / min, and then cooled to room temperature after a holding time of 8 hours to remove additives and other organic matter in the target blank.
[0123] (9) The target blank obtained in step (8) is placed in a sintering furnace for sintering in an oxygen atmosphere at a heating rate of 1°C / min. The temperature is raised to 1650°C and then kept at this temperature for 10 hours to obtain a barium-doped indium tin zinc oxide target.
[0124] Comparative Example 3 (1) Weigh indium oxide, tin oxide, zinc oxide, and barium oxide powders in a mass ratio of 80:10:2:8 and set aside.
[0125] (2) Add a certain amount of pure water into the slurry barrel, and add the tin oxide and zinc oxide powders weighed in step (1) and PVP into the slurry barrel in sequence for pre-dispersion. The dispersion time is 30 min and the dispersion speed is 100 rpm, wherein PVP accounts for 4% of the total mass of the added tin oxide powder, zinc oxide powder, pure water and PVP.
[0126] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 r / min to obtain slurry 1 with a solid content of 68%.
[0127] (3) Add barium oxide powder and PVP to slurry 1 for dispersion, the dispersion time is 30 minutes, and the dispersion speed is 100 rpm. PVP accounts for 4% of the total mass of the added barium oxide powder and PVP.
[0128] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 rpm to obtain slurry 2 with a solid content of 68%.
[0129] (4) Add indium oxide powder and PVP to slurry 2 for dispersion, with a dispersion time of 30 min and a dispersion speed of 100 rpm. PVP accounts for 4% of the total mass of the added indium oxide powder and PVP.
[0130] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 12 h and the grinding speed was 1500 rpm to obtain slurry three with a solid content of 68%.
[0131] (5) PVA was added to slurry 3 and pre-dispersed. The pre-dispersion time was 30 min and the dispersion speed was 100 rpm. The binder accounted for 10% of the mass of all the added substances.
[0132] The slurry was then pumped into a sand mill using a pneumatic diaphragm pump for grinding. The grinding time was 2 h and the grinding speed was 1500 rpm to obtain slurry 4 with a solid content of 68%.
[0133] (6) The slurry 4 is fed into a spray drying tower for spray granulation, and then mixed and sieved to obtain an indium tin zinc oxide mixed powder. The air outlet temperature is 75°C and the atomizer frequency is 120 Hz.
[0134] (7) The mixed powder obtained in step (6) is molded by molding and then cold isostatic pressing to obtain a barium-doped indium tin zinc oxide target blank.
[0135] (8) The target blank obtained in step (7) is placed in a sintering furnace for degreasing heat treatment. In an air atmosphere, the temperature is controlled at 500°C at a heating rate of 0.5 / min, and then cooled to room temperature after a holding time of 8 hours to remove additives and other organic matter in the target blank.
[0136] (9) The target blank obtained in step (8) is placed in a sintering furnace for sintering in an oxygen atmosphere at a heating rate of 1°C / min. The temperature is raised to 1500°C and then kept at this temperature for 10 hours to obtain a barium-doped indium tin zinc oxide target.
[0137] Comparative Example 4 (1) Weigh indium oxide, tin oxide, zinc oxide, and barium oxide powders in a mass ratio of 87:10:2:1 and set aside.
[0138] (2) Add a certain amount of pure water into the slurry barrel, and add the tin oxide and zinc oxide powders weighed in step (1) and PVP into the slurry barrel in sequence for pre-dispersion. The dispersion time is 30 min and the dispersion speed is 100 rpm, wherein PVP accounts for 4% of the total mass of the added tin oxide powder, zinc oxide powder, pure water and PVP.
[0139] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 r / min to obtain slurry 1 with a solid content of 65%.
[0140] (3) Add barium oxide powder and PVP to slurry 1 for dispersion, the dispersion time is 30 minutes, and the dispersion speed is 100 rpm. PVP accounts for 4% of the total mass of the added barium oxide powder and PVP.
[0141] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 rpm to obtain slurry 2 with a solid content of 65%.
[0142] (4) Add indium oxide powder and PVP to slurry 2 for dispersion, with a dispersion time of 30 min and a dispersion speed of 100 rpm. PVP accounts for 4% of the total mass of the added indium oxide powder and PVP.
[0143] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 12 h and the grinding speed was 1500 rpm to obtain slurry three with a solid content of 65%.
[0144] (5) PVA was added to slurry 3 and pre-dispersed. The pre-dispersion time was 30 min and the dispersion speed was 100 rpm. The binder accounted for 10% of the mass of all the added substances.
[0145] The slurry was then pumped into a sand mill using a pneumatic diaphragm pump for grinding. The grinding time was 2 h and the grinding speed was 1500 rpm to obtain slurry 4 with a solid content of 65%.
[0146] (6) The slurry 4 is fed into a spray drying tower for spray granulation, and then mixed and sieved to obtain an indium tin zinc oxide mixed powder. The air outlet temperature is 75°C and the atomizer frequency is 120 Hz.
[0147] (7) The mixed powder obtained in step (6) is molded by molding and then cold isostatic pressing to obtain a barium-doped indium tin zinc oxide target blank.
[0148] (8) The target blank obtained in step (7) is placed in a sintering furnace for degreasing heat treatment. In an air atmosphere, the temperature is controlled at 500°C at a heating rate of 0.5 / min, and then cooled to room temperature after a holding time of 8 hours to remove additives and other organic matter in the target blank.
[0149] (9) The target blank obtained in step (8) is placed in a sintering furnace for sintering in an oxygen atmosphere at a heating rate of 1°C / min. The temperature is raised to 1500°C and then kept at this temperature for 10 hours to obtain a barium-doped indium tin zinc oxide target.
[0150] Comparative Example 5 (1) Weigh indium oxide, tin oxide, zinc oxide, and barium oxide powders in a mass ratio of 88:10:2:0 and set aside.
[0151] (2) Add a certain amount of pure water into the slurry barrel, and add the tin oxide and zinc oxide powders weighed in step (1) and PVP into the slurry barrel in sequence for pre-dispersion. The dispersion time is 30 min and the dispersion speed is 100 rpm, wherein PVP accounts for 4% of the total mass of the added tin oxide powder, zinc oxide powder, pure water and PVP.
[0152] The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding. The grinding time was 6 hours and the grinding speed was 1500 r / min to obtain slurry 1 with a solid content of 70%.
[0153] (3) Indium oxide powder and PVP were added to slurry 1 for dispersion, the dispersion time was 30 min, and the dispersion speed was 100 rpm. The obtained slurry was pumped into a sand mill by a pneumatic diaphragm pump for grinding, the grinding time was 12 h, and the grinding speed was 1500 rpm to obtain slurry 3 with a solid content of 70%. PVP accounted for 4% of the total mass of the added indium oxide powder and PVP.
[0154] (4) PVA was added to slurry 3' and pre-dispersed for 30 min at a dispersing speed of 100 rpm. The slurry was then pumped into a sand mill for grinding for 2 h at a grinding speed of 1500 rpm to obtain slurry 4 with a solid content of 70%. The binder accounted for 10% of the mass of all the added substances.
[0155] (5) The slurry 4' is fed into a spray drying tower for spray granulation, and then mixed and sieved to obtain an indium tin zinc oxide mixed powder. The air outlet temperature is 75°C and the atomizer frequency is 120 Hz.
[0156] (6) The mixed powder obtained in step (5) is molded by molding and then cold isostatic pressing to obtain a barium-doped indium tin zinc oxide target blank.
[0157] (7) The target blank obtained in step (6) is placed in a sintering furnace for degreasing heat treatment. In an air atmosphere, the temperature is controlled at 500°C at a heating rate of 0.5 / min, and after a holding time of 8 hours, it is cooled to room temperature to remove additives and other organic matter in the target blank.
[0158] (8) The target blank obtained in step (7) is placed in a sintering furnace for sintering in an oxygen atmosphere at a heating rate of 1°C / min. The temperature is raised to 1500°C and then kept at this temperature for 10 hours to obtain a barium-doped indium tin zinc oxide target.
[0159] Test Example The relative density and resistance of the target materials obtained in the examples and comparative examples were tested.
[0160] The target materials obtained in the embodiment and the comparative example were subjected to DC magnetron sputtering to form films, and the sputtering process parameters were as follows: sputtering power 10 kW, Ar amount: 294 Sccm, Ar-H2 amount: 606 Sccm, O2 amount: 22 Sccm, H2 amount: 17 Sccm. The mobility and transmittance of the prepared films were tested.
[0161] The above data are shown in Table 1.
[0162] It can be seen that: When the doping amount of barium oxide is 2-4%, the relative density and resistance of the target material are improved, and after sputtering, the film performance is also significantly better than other doping concentrations. The target material of the present application is relatively sensitive to the sintering temperature during preparation, and exhibits the best comprehensive performance at 1400° C. to 1600° C. It can be seen from the comparative examples that if the sintering temperature is too high or too low, the performance of the target material finally obtained is far from meeting the actual needs.
[0163] Table 1 The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the scope of the present invention.
Claims
1. A method for preparing a barium-doped indium tin zinc oxide target, characterized in that: The following steps are involved: (1) Weigh indium oxide powder, tin oxide powder, zinc oxide powder, and barium oxide powder in a mass ratio of 84-92.5:5-10:0.5-2:2-4; (2) Pour zinc oxide powder, tin oxide powder and a first dispersant into a container containing pure water, disperse them uniformly, and then perform wet grinding to obtain slurry 1; (3) adding barium oxide powder and a second dispersant to slurry 1, dispersing them uniformly, and then wet grinding them to obtain slurry 2; (4) adding indium oxide powder and a third dispersant to slurry 2, dispersing them uniformly, and then wet grinding them to obtain slurry 3; (5) adding a binder to slurry 3, dispersing the slurry evenly, and then wet grinding the slurry to obtain slurry 4; (6) using slurry 4 as a raw material to perform spray granulation to obtain barium-doped indium tin zinc oxide powder; (7) using barium-doped indium tin zinc oxide powder as a raw material for pressing and molding to obtain a barium-doped indium tin zinc oxide target blank; (8) The barium-doped indium tin zinc oxide target blank is subjected to degreasing heat treatment and sintering heat treatment in sequence to obtain a barium-doped indium tin zinc oxide target material.
2. The preparation method according to claim 1, characterized in that In step (1), the purity of the tin oxide is 4N; the purity of the tin oxide is 4N; the purity of the zinc oxide is 4N; and the purity of the barium oxide powder is 4N.
3. The preparation method according to claim 1, characterized in that: The first dispersant, the second dispersant or the third dispersant is at least one of polyvinyl pyrrolidone, sodium dodecylbenzene sulfonate and sodium hexadecylbenzene sulfonate; Preferably, the binder is at least one of a mixture of polyvinyl alcohol and polyethylene glycol, polyvinyl alcohol, and polyvinyl butyral.
4. The preparation method according to claim 1, characterized in that: The first dispersant accounts for 1-5% of the total mass of the tin oxide powder, the zinc oxide powder, the pure water and the first dispersant; Preferably, the second dispersant accounts for 1-15% of the total mass of the barium oxide powder and the second dispersant; Preferably, the third dispersant accounts for 1-15% of the total mass of the indium oxide powder and the third dispersant; Preferably, the binder accounts for 5-15% of the total mass of the tin oxide powder, the indium oxide powder, the barium oxide powder, the zinc oxide powder, the first dispersant, the second dispersant, the third dispersant and the binder.
5. The preparation method according to claim 1, characterized in that: The solid content of the slurry one is 60-70%; the solid content of the slurry two is 60-70%; the solid content of the slurry three is 60-70%; the solid content of the slurry four is 60-70%.
6. The preparation method according to claim 1, characterized in that: In step (6), a spray drying tower is used for spray granulation; the outlet air temperature of the spray drying tower is 70-85° C., and the atomizer frequency is 110-130 Hz.
7. The preparation method according to claim 1, characterized in that: In step (7), compression molding is performed by cold isostatic pressing after molding.
8. The preparation method according to claim 1, characterized in that: In step (8), the degreasing heat treatment is as follows: in an air atmosphere, the temperature is raised to 400°C~600°C at a heating rate of 0.1~0.5°C / min, and the temperature is kept for 6~12 hours.
9. The preparation method according to claim 1, characterized in that: In step (8), the sintering heat treatment is as follows: in an oxygen atmosphere, the temperature is raised to 1400°C~1600°C at a heating rate of 0.5~1.5°C / min, and the temperature is kept for 8~12 hours.
10. A barium-doped indium tin zinc oxide target prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Sputtering target and method for manufacturing oxide sintered body
CN101316944A
Target for forming transparent conductive film, method of manufacturing the target, and method of manufacturing transparent conductive film
CN108220893A
Indium zinc oxide target material and preparation method thereof
CN116162908A
In2O3-ZnO-BASED SPUTTERING TARGET AND OXIDE CONDUCTIVE FILM
JP2013001919A
Transparent conductive oxid film and indium-zinc composite oxid and sintered material