Ceramic substrate and preparation method thereof

By setting the ceramic substrate's green ceramic belt orientation consistent and adopting isostatic molding and staged sintering processes, the layering problem during sintering of ceramic substrates is solved, the sintering yield and dielectric performance are improved, and the high quality of ceramic substrates is ensured preparation.

CN118930231APending Publication Date: 2024-11-12GUANGDONG HUANBO NEW MATERIAL CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410905508.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing ceramic substrates are prone to stratification during sintering, resulting in low sintering yield.

Method used

By setting the first and second surfaces of the multiple raw porcelain belts to the same orientation, stacking is performed, and vacuum isostatic molding and staged sintering are adopted to ensure a good interface combination between the various layers of raw porcelain belts. .

Benefits of technology

It effectively improves the layering problem of ceramic substrates during sintering, improves the sintering yield to 100%, and improves the dielectric performance and appearance quality of ceramic substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004931952400000091
    Figure BDA0004931952400000091
Patent Text Reader

Abstract

The invention discloses a ceramic substrate and a preparation method thereof, and relates to the technical field of electronic packaging materials, the ceramic substrate comprises a plurality of green tapes which are arranged in a laminated manner, each green tape has a first surface and a second surface which are opposite to each other, and the first surfaces / second surfaces of the plurality of green tapes face the same direction. The directions of the green tapes of the ceramic substrate provided by the invention are consistent, so that the green tapes have good interface bonding, and the phenomenon that layering is easy to occur during sintering is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electronic packaging materials, and in particular to a ceramic substrate and a preparation method thereof. Background Art

[0002] At present, the commonly used electronic packaging materials mainly include plastic substrates, metal substrates, ceramic substrates and composite substrates. Among them, ceramic substrates have excellent electrical insulation properties, high thermal conductivity, excellent soft soldering performance and high adhesion strength, and can be etched with various patterns like PCB boards, and have a large current carrying capacity. Therefore, ceramic substrates are widely used in high-power power semiconductor modules, power control circuits, automotive electronics, aerospace, military electronic components, and solar panel components.

[0003] However, the existing ceramic substrates have the problem of easy delamination during sintering, resulting in a low sintering yield of the product. Summary of the invention

[0004] The main purpose of the present invention is to provide a ceramic substrate and a preparation method thereof, aiming to improve the delamination problem existing in the ceramic substrate during sintering.

[0005] To achieve the above object, the ceramic substrate provided by the present invention comprises a plurality of stacked green ceramic tapes, each of which has a first surface and a second surface opposite to each other, and the first surfaces / second surfaces of the plurality of green ceramic tapes are oriented in the same direction.

[0006] In one embodiment, the green tape has a thickness of 30-60 μm.

[0007] In one embodiment, the thickness of the ceramic substrate is 0.1-2.0 mm.

[0008] The present invention also provides a method for preparing a ceramic substrate, comprising the following steps:

[0009] A plurality of green porcelain tapes are stacked, each of the green porcelain tapes having a first surface and a second surface opposite to each other, and the first surfaces / second surfaces of the plurality of green porcelain tapes are controlled to be oriented in the same direction;

[0010] The stacked green porcelain tapes are evacuated and then isostatically pressed;

[0011] The ceramic substrate can be obtained by sintering the green ceramic tape formed by isostatic pressing.

[0012] In one embodiment, the parameters of isostatic pressing are: temperature 50-80° C., pressure 50-100 MPa, and holding time 10-20 min.

[0013] In one embodiment, the sintering includes a first stage sintering and a second stage sintering;

[0014] The parameters of the first stage sintering are: from room temperature to the first sintering temperature, the heating rate is 0.1-0.5°C / min, the holding time is 4-6h, and the first sintering temperature is 500-1000°C; and / or,

[0015] The parameters of the second stage sintering are: from the first sintering temperature to the second sintering temperature, the heating rate is 0.5-1°C / min, the holding time is 2-4h, and the second sintering temperature is 1450-1600°C.

[0016] In one embodiment, the method for preparing the ceramic substrate further includes making a green ceramic tape, which specifically includes the following steps:

[0017] Alumina powder and a dispersant are added to a solvent and ground and mixed to obtain slurry I, and then a plasticizer and a binder are added to the slurry I and ground and mixed to obtain slurry II;

[0018] Slurry II was tape cast to form a green tape.

[0019] In one embodiment, the amount of aluminum oxide powder added is 40wt%-60wt%, the amount of dispersant added is 1wt%-3wt%, the amount of plasticizer added is 2wt%-5wt%, the amount of binder added is 5wt%-10wt%, and the balance is solvent.

[0020] In one embodiment, the purity of the aluminum oxide powder is greater than 99%, and the particle size D 50 0.5-1.0 μm; and / or,

[0021] The dispersant is triolein; and / or,

[0022] The plasticizer is selected from at least one of dioctyl phthalate and polyethylene glycol; and / or,

[0023] The binder is polyvinyl butyral; and / or,

[0024] The solvent is a mixture of alcohol and ester, and the mass ratio of the alcohol to the ester is 1-3:7-9.

[0025] In one embodiment, the alcohol is selected from at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol, and isobutanol; and / or,

[0026] The ester is selected from at least one of ethyl acetate, methyl acetate, propyl acetate and butyl acetate.

[0027] The technical solution of the present invention sets the directions of the various green porcelain tapes of the ceramic substrate to be consistent, that is, the first surfaces / second surfaces of the multiple green porcelain tapes are set in the same direction, so that the layers of green porcelain tapes can have good interface bonding. Because during the casting process of the green porcelain tape, the drying and volatilization rates of the solvent and the like in the surface facing the carrier film surface and the surface facing the air are inconsistent, and the surface facing the carrier film surface has greater viscosity. When the directions of the multiple green porcelain tapes are set to be consistent, the surface of each green porcelain tape facing the carrier film surface can be bonded to the surface of the adjacent green porcelain tape facing the air, thereby ensuring the bonding force between the interfaces and thereby improving the phenomenon of stratification that is easy to occur during sintering. DETAILED DESCRIPTION

[0028] It should be noted that the meaning of "and / or" in the present invention includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or solutions that satisfy both A and B. "At least one" in the present invention means one or more, and "more than one" means two or more.

[0029] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.

[0030] "Scope" disclosed in the present invention is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3,4 and 5 are listed, the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present invention, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0031] If not otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0032] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0033] In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the fact that ordinary technicians in the field can implement it. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0034] In recent years, with the vigorous development of the microelectronics packaging industry, electronic packaging technology has developed in the direction of miniaturization, high density, multi-power and high reliability, and electronic packaging materials have gradually become an important industrial field with high technology content and high economic benefits. Currently, the commonly used electronic packaging materials are mainly divided into four categories: plastic substrates, metal substrates, ceramic substrates and composite substrates. Among them, ceramic substrates have excellent electrical insulation properties, high thermal conductivity, excellent soft soldering performance and high adhesion strength, and can be etched with various patterns like PCB boards, and have great current carrying capacity. Therefore, ceramic substrates are widely used in high-power power semiconductor modules, power control circuits, automotive electronics, aerospace, military electronic components, and solar panel components.

[0035] Existing ceramic substrates use a conventional lamination method, which results in poor interface bonding between the layers and easy delamination during sintering.

[0036] To this end, the present invention provides a ceramic substrate, comprising a plurality of stacked green ceramic tapes, each of which has a first surface and a second surface opposite to each other, and the first surfaces / second surfaces of the plurality of green ceramic tapes are oriented in the same direction.

[0037] The technical solution of the present invention sets the directions of the layers of green porcelain tapes of the ceramic substrate to be consistent, that is, the first surfaces / second surfaces of the multiple green porcelain tapes are set to the same direction. Specifically, the first surfaces of the multiple layers of green porcelain tapes can be set to face upward and the second surfaces can be set to face downward. In this way, the layers of green porcelain tapes can have good interface bonding. Because during the casting process of the green porcelain tape, the drying and volatilization rates of the solvent and the like in the surface facing the carrier film surface (first surface) and the surface facing the air (second surface) are inconsistent, and the surface facing the carrier film surface has greater viscosity. When the directions of the multiple green porcelain tapes are set to be consistent, the surface of each green porcelain tape facing the carrier film surface can be bonded to the surface of the adjacent green porcelain tape facing the air, thereby ensuring the bonding force between the interfaces and thereby improving the phenomenon of stratification that is easy to occur during sintering.

[0038] In an embodiment of the present invention, the thickness of the green porcelain tape is 30-60 μm.

[0039] In an embodiment of the present invention, the thickness of the ceramic substrate is 0.1-2.0 mm.

[0040] The present invention also provides a method for preparing a ceramic substrate, comprising the following steps:

[0041] A plurality of green porcelain tapes are stacked, each of the green porcelain tapes having a first surface and a second surface opposite to each other, and the first surfaces / second surfaces of the plurality of green porcelain tapes are controlled to be oriented in the same direction;

[0042] The stacked green porcelain tapes are evacuated and then isostatically pressed;

[0043] The ceramic substrate can be obtained by sintering the green ceramic tape formed by isostatic pressing.

[0044] In the embodiment of the present invention, the parameters of isostatic pressing are: temperature 50-80°C, pressure 50-100 MPa, and holding time 10-20 min. This parameter is the optimal isostatic pressing condition, which can further improve the problem of product delamination after sintering.

[0045] In an embodiment of the present invention, the sintering includes a first stage sintering and a second stage sintering;

[0046] The parameters of the first stage sintering are: from room temperature to the first sintering temperature, the heating rate is 0.1-0.5°C / min, the holding time is 4-6h, and the first sintering temperature is 500-1000°C; and / or,

[0047] The parameters of the second stage sintering are: from the first sintering temperature to the second sintering temperature, the heating rate is 0.5-1°C / min, the holding time is 2-4h, and the second sintering temperature is 1450-1600°C.

[0048] The first stage sintering is a pre-sintering process, which can ensure that the green porcelain belt is completely degreased on the one hand, and on the other hand, it can prevent the gas generated by the combustion of residual organic matter from forming gaps or stratification inside; the second stage sintering is a sintering process, and the appropriate heating rate avoids stress concentration inside, thereby avoiding stratification.

[0049] In an embodiment of the present invention, the method for preparing a ceramic substrate further includes making a green ceramic tape, which specifically includes the following steps:

[0050] Alumina powder and a dispersant are added to a solvent and ground and mixed to obtain slurry I, and then a plasticizer and a binder are added to the slurry I and ground and mixed to obtain slurry II;

[0051] Slurry II was tape cast to form a green tape.

[0052] In an embodiment of the present invention, the addition amount of alumina powder is 40wt%-60wt%, the addition amount of dispersant is 1wt%-3wt%, the addition amount of plasticizer is 2wt%-5wt%, the addition amount of binder is 5wt%-10wt%, and the balance is solvent.

[0053] In the embodiment of the present invention, the purity of the aluminum oxide powder is greater than 99%, and the particle size D 50 is 0.5-1.0 μm; and / or, the dispersant is triolein; and / or, the plasticizer is selected from at least one of dioctyl phthalate and polyethylene glycol; and / or, the binder is polyvinyl butyral; and / or, the solvent is a mixture of alcohol and ester, and the mass ratio of alcohol to ester is 1-3:7-9.

[0054] It should be noted that the particle size D 50 The median diameter or median particle size refers to the particle size corresponding to when the cumulative particle size distribution percentage of the sample reaches 50%. Taking the embodiment of the present invention as an example, in the alumina powder, the particles with a particle size greater than 0.5-1.0 μm account for 50%, and the particles with a particle size less than 0.5-1.0 μm also account for 50%.

[0055] The alumina powder in the embodiment of the present invention is of submicron grade, so that after sintering, the dielectric properties of the ceramic substrate can be improved and defects such as gray spots and white spots on the appearance of the ceramic substrate can be ensured.

[0056] In an embodiment of the present invention, the alcohol is selected from at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol, and isobutanol; and / or the ester is selected from at least one of ethyl acetate, methyl acetate, propyl acetate, and butyl acetate.

[0057] The following describes the invention in conjunction with specific embodiments.

[0058] Example 1

[0059] The method for preparing a ceramic substrate comprises the following steps:

[0060] (1) Weigh 1000 g of alumina powder (purity 99.98%, particle size D 50 0.6 μm), 20 g of triolein, 80 g of dioctyl phthalate, 100 g of polyvinyl butyral, and 800 g of solvent (including 240 g of ethanol and 560 g of ethyl acetate);

[0061] (2) adding the weighed alumina powder to the solvent, and then adding triolein, grinding and mixing by a ball mill for 24 hours to obtain slurry I; then adding dioctyl phthalate and polyvinyl butyral to slurry I, grinding and mixing by a ball mill for 24 hours to obtain slurry II;

[0062] (3) Casting slurry II into a 60 μm thick green porcelain tape;

[0063] (4) laminating the green porcelain tape formed by tape casting to a thickness of 0.5 mm, controlling the laminating direction to be consistent, specifically setting the first surface of the green porcelain tape to face upward and the second surface to face downward, then evacuating the laminated product, and placing it in an isostatic press for isostatic pressing, and the parameters of the isostatic pressing are: temperature 80° C., pressure 100 MPa, and holding time 10 min;

[0064] (5) First stage sintering: heating from room temperature to 500 °C, heating rate 0.1 °C / min, holding time 2 h;

[0065] (6) Second stage sintering: heating from 500 °C to 1530 °C at a heating rate of 0.5 °C / min, keeping at this temperature for 4 h, and then cooling to room temperature at a cooling rate of 1 °C / min;

[0066] (7) After sintering, the ceramic substrate can be obtained.

[0067] Example 2

[0068] Different from Example 1, the isostatic pressing temperature in this example is 60°C, the pressure is 50 MPa, the heating rate of the first stage sintering is 0.2°C / min, and the heating rate of the second stage sintering is 1°C / min; the remaining steps are the same as in Example 1.

[0069] Example 3

[0070] The difference from Example 1 is that the isostatic pressing pressure in this example is 80 MPa, and the remaining steps are the same as those in Example 1.

[0071] Example 4

[0072] The difference from Example 1 is that the isostatic pressing temperature in this embodiment is 65° C. and the pressure is 80 MPa, and the remaining steps are the same as those in Example 1.

[0073] Example 5

[0074] Different from Example 1, the isostatic pressing pressure in this example is 80 MPa and the holding time is 15 min. The remaining steps are the same as those in Example 1.

[0075] Example 6

[0076] The difference from Example 1 is that in this example, the green porcelain tape formed by tape casting is laminated to a thickness of 1.0 mm, and the remaining steps are the same as those in Example 1.

[0077] Example 7

[0078] The difference from Example 1 is that in this example, the green porcelain tape formed by tape casting is laminated to a thickness of 2.0 mm, and the remaining steps are the same as those in Example 1.

[0079] Comparative Example 1

[0080] Different from Example 1, the stacking directions of the green porcelain tapes in this comparative example are inconsistent, that is, the directions of the green porcelain tapes are arranged to be alternately distributed, specifically, the first surface of the first layer of green porcelain tapes is arranged to face upward and the second surface is arranged to face downward, the second surface of the second layer of green porcelain tapes is arranged to face upward and the first surface is arranged to face downward, the first surface of the third layer of green porcelain tapes is arranged to face upward and the second surface is arranged to face downward, and so on. The remaining steps are the same as those in Example 1.

[0081] Comparative Example 2

[0082] Different from Example 1, the isostatic pressing pressure in this comparative example is 40 MPa, and the remaining steps are the same as those in Example 1.

[0083] Comparative Example 3

[0084] The difference from Example 1 is that the isostatic pressing pressure in this comparative example is 120 MPa, and the remaining steps are the same as those in Example 1.

[0085] Comparative Example 4

[0086] Different from Example 3, the isostatic pressing temperature in this comparative example is 45°C, and the remaining steps are the same as those in Example 3.

[0087] Comparative Example 5

[0088] The difference from Example 3 is that the isostatic pressing temperature in this comparative example is 85° C., and the remaining steps are the same as those in Example 3.

[0089] Comparative Example 6

[0090] The difference from Example 3 is that the holding time of the isostatic pressing in this comparative example is 8 minutes, and the other steps are the same as those in Example 3.

[0091] Comparative Example 7

[0092] The difference from Example 3 is that the holding time of the isostatic pressing in this comparative example is 22 minutes, and the other steps are the same as those in Example 3.

[0093] Comparative Example 8

[0094] Different from Example 3, the heating rate of the first stage in this comparative example is 0.6°C / min, and the remaining steps are the same as those in Example 3.

[0095] Comparative Example 9

[0096] Different from Example 3, the heating rate of the first stage in this comparative example is 1.0°C / min, and the remaining steps are the same as those in Example 3.

[0097] Comparative Example 10

[0098] Different from Example 3, the heating rate of the first stage in this comparative example is 0.5°C / min, and the remaining steps are the same as those in Example 3.

[0099] Comparative Example 11

[0100] Different from Example 3, the heating rate of the second stage in this comparative example is 1.2°C / min, and the remaining steps are the same as those in Example 3.

[0101] Comparative Example 12

[0102] Different from Example 3, the heating rate of the second stage in this comparative example is 1.5°C / min, and the remaining steps are the same as those in Example 3.

[0103] Comparative Example 13

[0104] Different from Example 3, the heating rate of the first stage in this comparative example is 2.0°C / min, and the remaining steps are the same as those in Example 3.

[0105] Comparative Example 14

[0106] Different from Example 1, the stacking direction of the green porcelain tape in this comparative example is inconsistent (refer to the settings in Comparative Example 1 for details), the isostatic pressing temperature is 45°C, the pressure is 40MPa, the holding time is 8min, the first stage heating rate is 0.6°C / min, and the second stage heating rate is 1.2°C / min, and the remaining steps are the same as in Example 1.

[0107] The appearance of the ceramic substrates prepared in the above-mentioned Examples 1-7 and Comparative Examples 1-14 was evaluated. Specifically, 360 ceramic substrates were prepared in the same batch under various experimental conditions. The appearance of the ceramic substrates was then observed under light transmission conditions. The ratio of stratified ceramic substrates to the total ceramic substrates was calculated to obtain the stratification ratio. The specific results are shown in the following table.

[0108] Table 1 Experimental parameters and results in Examples 1-7 and Comparative Examples 1-14

[0109]

[0110] It can be seen from the above table that when the orientations of the green ceramic tapes of each layer are set to be consistent and the optimal isostatic pressing and sintering conditions are adopted, the obtained ceramic substrates have no delamination and the sintering yield reaches 100%.

[0111] By comparing Example 1 and Comparative Example 1, it can be seen that, on the basis of other conditions being the same, when only the orientation of each raw ceramic tape is set to be consistent, the stratification ratio is reduced from 51% to zero, indicating that the consistent stacking direction of the present invention can effectively improve the stratification problem during the sintering of the ceramic substrate.

[0112] By comparing Example 3 with Comparative Examples 2 and 3, it can be seen that when the isostatic pressing pressure is lower or higher than the optimal range of 50-100 MPa in the present invention, the ceramic substrate will be delaminated. This is because when the pressure is too low, the layers cannot be tightly combined, resulting in delamination. If the pressure is too high, elastic aftereffect will occur, resulting in delamination.

[0113] By comparing Example 3 with Comparative Examples 4 and 5, it can be seen that when the temperature of isostatic pressing is lower than or higher than the optimal range of 50-80°C of the present invention, stratification will occur on the ceramic substrate. This is because when the temperature is too low, the softening temperature of the binder is not reached, and the interfaces of the layers are not tightly bonded during pressing, resulting in stratification. When the temperature is higher than the softening temperature of the binder, the flow of the binder will cause uneven density of the substrate, thereby inducing stratification.

[0114] By comparing Example 3 with Comparative Examples 6 and 7, it can be seen that when the holding time of isostatic pressing is lower than or higher than the optimal range of 10-20 min of the present invention, stratification will occur on the ceramic substrate. This is because the holding time is too short and the layers cannot be tightly combined, resulting in stratification. When the holding time is too long, elastic aftereffect will occur, leading to stratification.

[0115] Comparing Example 3 with Comparative Examples 8, 9, and 10, it can be seen that when the heating rate in the first stage is higher than the optimal range of 0.1-0.5°C / min of the present invention, the ceramic substrate will be delaminated; comparing Example 4 with Comparative Examples 11, 12, and 13, it can be seen that when the heating rate in the second stage is higher than the optimal range of 0.5-1.0°C / min of the present invention, the ceramic substrate will be delaminated. This is because a too fast heating rate will cause stress concentration inside the substrate, which will cause delamination.

[0116] The above description is only an exemplary embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the technical concept of the present invention, or direct / indirect application in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A ceramic substrate, characterized in that: The ceramic substrate includes a plurality of stacked green ceramic tapes, each of which has a first surface and a second surface that are opposite to each other, and the first surfaces / second surfaces of the plurality of green ceramic tapes are oriented in the same direction.

2. The ceramic substrate according to claim 1, characterized in that The thickness of the green porcelain tape is 30-60 μm.

3. The ceramic substrate according to claim 1 or 2, characterized in that: The thickness of the ceramic substrate is 0.1-2.0 mm.

4. A method for preparing a ceramic substrate, characterized in that: The following steps are involved: Laying down a plurality of green porcelain tapes, each of the green porcelain tapes having a first surface and a second surface opposite to each other, and controlling the first surfaces / second surfaces of the plurality of green porcelain tapes to face the same direction; The stacked green porcelain tapes are evacuated and then isostatically pressed; The ceramic substrate can be obtained by sintering the green ceramic tape formed by isostatic pressing.

5. The method for preparing a ceramic substrate according to claim 4, characterized in that: The parameters of the isostatic pressing are: temperature 50-80°C, pressure 50-100MPa, and holding time 10-20min.

6. The method for preparing a ceramic substrate according to claim 4, characterized in that: The sintering includes a first stage sintering and a second stage sintering; The parameters of the first stage sintering are: from room temperature to the first sintering temperature, the heating rate is 0.1-0.5°C / min, the holding time is 4-6h, and the first sintering temperature is 500-1000°C; and / or, The parameters of the second stage sintering are: from the first sintering temperature to the second sintering temperature, the heating rate is 0.5-1°C / min, the holding time is 2-4h, and the second sintering temperature is 1450-1600°C.

7. The method for preparing a ceramic substrate according to claim 4, characterized in that: The method for preparing the ceramic substrate also includes the production of a green ceramic tape, which specifically includes the following steps: Alumina powder and a dispersant are added to a solvent and ground and mixed to obtain slurry I, and then a plasticizer and a binder are added to the slurry I and ground and mixed to obtain slurry II; The slurry II was tape cast to form a green tape.

8. The method for preparing a ceramic substrate according to claim 7, characterized in that: The addition amount of the alumina powder is 40wt%-60wt%, the addition amount of the dispersant is 1wt%-3wt%, the addition amount of the plasticizer is 2wt%-5wt%, the addition amount of the binder is 5wt%-10wt%, and the balance is solvent.

9. The method for preparing a ceramic substrate according to claim 7 or 8, characterized in that: The purity of the aluminum oxide powder is greater than 99%, and the particle size D 50 0.5-1.0 μm; and / or, The dispersant is triolein; and / or, The plasticizer is selected from at least one of dioctyl phthalate and polyethylene glycol; and / or, The binder is polyvinyl butyral; and / or, The solvent is a mixture of alcohol and ester, and the mass ratio of the alcohol to the ester is 1-3:7-9.

10. The method for preparing a ceramic substrate according to claim 9, characterized in that: The alcohol is selected from at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol and isobutanol; and / or, The ester is selected from at least one of ethyl acetate, methyl acetate, propyl acetate and butyl acetate.

Citation Information

Patent Citations

  • Aluminum oxide ceramic substrate with high heat conductivity and preparation method thereof

    CN103408291A

  • Preparation method of ultrahigh-density ceramic biscuit

    CN112297189A

  • High-purity ultrathin high-strength aluminum oxide ceramic substrate as well as preparation method and application thereof

    CN114538900A