Preparation method of transparent aluminum oxide ceramic substrate

By grinding and screening alumina ceramic raw materials, combined with slow stirring and vacuum disposal technology, the problem of uneven density of alumina ceramic substrates is solved, the density uniformity and light transmittance of transparent alumina ceramic substrates are improved, and the density uniformity and light transmittance of transparent alumina ceramic substrates are reduced. The sintering temperature is improved, and the production quality and energy efficiency are improved.

CN118930234AInactive Publication Date: 2024-11-12FUJIAN HUAQING ELECTRONICS MATERIAL TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411130501.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing alumina ceramic substrates have uneven density during the molding process, resulting in poor quality.

Method used

通过对透明氧化铝陶瓷原料进行研磨和筛选,制备均匀粒径的粉体料浆,并在模具中进行缓慢搅拌和真空排胶,结合上下翻转固化处理,随后进行煅烧和烧结处理,采用高纯纳米氧化铝和氧化镁掺杂以抑制晶粒生长,引入烧结助剂以降低烧结温度。

Benefits of technology

The uniformity of ceramic substrate density is improved, light transmittance is improved, sintering temperature is reduced, energy consumption is reduced, sintering shrinkage and controllability are improved, and production quality is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of aluminum oxide ceramic substrates, and discloses a preparation method of a transparent aluminum oxide ceramic substrate. The method comprises the following steps: 1, preparing a transparent alumina ceramic raw material, pouring the prepared raw material into a grinding device, and starting the grinding device to perform multi-stage grinding and crushing treatment on the raw material to obtain raw material powder; 2, uniformly mixing the obtained raw material powder, and filtering through a 50-60-mesh sieve; the preparation method comprises the following steps: grinding and screening a transparent alumina ceramic raw material to obtain powder slurry with uniform particle size, slowly stirring the slurry when the slurry is poured into a mold, carrying out drying and glue discharging on the prefabricated slurry to obtain an intermediate blank, and overturning up and down to cure the blank so that the blank has a certain condensation degree. And the situation that materials with high specific gravity are precipitated in the slurry curing process is avoided, so that the density difference of the finally prepared ceramic substrate is small, the density is more uniform, and the production quality of the aluminum oxide ceramic substrate is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alumina ceramic substrates, and in particular to a method for preparing a transparent alumina ceramic substrate. Background Art

[0002] At present, the technology of microelectronics industry is developing rapidly, and electronic devices and electronic equipment are developing towards high integration and miniaturization, and the performance requirements for substrates are getting higher and higher. Due to the remarkable characteristics of alumina substrates such as excellent insulation performance, good thermal conductivity, low thermal expansion coefficient and strong mechanical strength, they are widely used in the field of electronic industry packaging. At present, most of the alumina substrates on the market are mainly 96 alumina substrates. Although they are widely used in thick film integrated circuits, LED packaging and other fields, high-purity alumina substrates are required for input and output substrates for high-frequency devices, substrates for optical communication devices, substrates for relays, etc., in order to achieve low loss.

[0003] When the existing alumina ceramic substrate is formed, the material with high specific gravity in the ceramic slurry is easily deposited at the bottom of the mold. After solidification and forming, the density of the green body near the bottom of the mold is high, and the density of the green body near the top of the mold is low. The overall density difference of the green body is large, resulting in a large density difference and uneven density of the ceramic substrate finally obtained, resulting in poor quality of the alumina ceramic substrate. Summary of the invention

[0004] In order to overcome the technical defects of the prior art, the present invention provides a method for preparing a transparent alumina ceramic substrate to solve the problem of poor quality of the alumina ceramic substrate mentioned in the above background technology.

[0005] The technical solution adopted by the present invention is: a method for preparing a transparent alumina ceramic substrate, comprising the following steps; Step 1: prepare transparent alumina ceramic raw materials, pour the prepared raw materials into a grinding device, start the grinding device to perform multi-stage grinding and crushing treatment on the raw materials to obtain raw material powder; Step 2: Mix the obtained raw material powders evenly, filter through a 50-60 mesh sieve, and use a stirring device to stir the powders to form a slurry with a certain viscosity, and then perform a degassing treatment; Step 3: Pour the degassed slurry into the mold, then seal the injection port, flip the lower side of the mold to the upper side, flip it 3-8 times, and perform vacuum debinding in a vacuum degreasing furnace to obtain a green body; Step 4: calcining and sintering the obtained green body to obtain the desired transparent alumina ceramic substrate.

[0006] Preferably, the transparent alumina ceramic raw material is as follows: 90-92 parts of alumina raw material, 3-10 parts of sintering aid, 3-5 parts of plasticizer, 2-3 parts of solvent, 1-2 parts of defoaming agent.

[0007] Preferably, the alumina raw material comprises alumina powder and magnesium oxide powder, and the mass ratio of the alumina powder to the magnesium oxide powder is (90-95):1.

[0008] Preferably, the sintering aid is a mixture of one or more of silicon dioxide, lithium carbonate, yttrium oxide, and cesium oxide, and the plasticizer is a mixture of one or more of polyethylene glycol, phthalate, and toluyl butyl phthalate.

[0009] Preferably, the solvent is a mixture of anhydrous ethanol and isopropanol, the mass ratio of the anhydrous ethanol to the isopropanol is 3:7, and the defoaming agent is one of tributyl phosphate or silicone oil.

[0010] Preferably, when the slurry in step 2 is poured into the mold, the slurry is stirred slowly at a stirring speed of 70-80 r / min.

[0011] Preferably, the mold in step 2 is kept for 2-3 minutes after being flipped, and the interval between each flipping is 5-10 minutes.

[0012] Preferably, the heating rate in the debinding process in step 2 is 50-60°C / h, the temperature is raised to 200-300°C and kept for 0.5-1h, so that the slurry is dried in a high temperature environment to ensure that the solvent evaporates slowly. After preliminary drying, the hardness of the slurry increases to form a green body.

[0013] Preferably, during the sintering, the green body is placed in a graphite crucible, placed in a sintering furnace with flowing nitrogen, the stable pressure is within 20-40KPa, the temperature is raised to 1400°C at a heating rate of 8-12°C / min, then the temperature is raised to 1600°C at a heating rate of 6-8°C / min, after keeping the temperature for 2-3h, the temperature is lowered to 1100°C at a cooling rate of 1-2°C / min, and then self-cooled to room temperature under flowing nitrogen to obtain a finished substrate.

[0014] Preferably, the method further comprises polishing and grinding the transparent alumina ceramic substrate to make its smoothness Ra less than 0.2 mm.

[0015] The preparation method of the transparent alumina ceramic substrate prepared by the present invention grinds and screens the transparent alumina ceramic raw material to obtain a powder slurry with uniform particle size, keeps the slurry slowly stirred when pouring it into a mold, obtains an intermediate embryo body by drying and debinding the prefabricated slurry, and then turns the embryo body upside down to solidify it so that it has a certain degree of coagulation, avoids precipitation of materials with high specific gravity during the solidification process of the slurry, makes the density difference of the finally prepared ceramic substrate small, the density is more uniform, and the production quality of the alumina ceramic substrate is improved.

[0016] The beneficial effects of the present invention are: The present invention adopts high-purity nano-alumina as raw material and dopes magnesium oxide to inhibit the rapid growth of ceramic grains at high temperature. The obtained transparent alumina ceramic sample has a smaller grain size, which makes it have a larger density and better light transmittance. At the same time, the introduction of sintering aids can reduce the sintering temperature of high-purity alumina ceramics, which not only reduces energy consumption but also improves sintering shrinkage and controllability. DETAILED DESCRIPTION

[0017] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] The present invention of this embodiment provides a method for preparing a transparent alumina ceramic substrate, comprising the following steps: Step 1: prepare transparent alumina ceramic raw materials, pour the prepared raw materials into a grinding device, start the grinding device to perform multi-stage grinding and crushing treatment on the raw materials to obtain raw material powder; Step 2: Mix the obtained raw material powders evenly, filter through a 50-60 mesh sieve, and use a stirring device to stir the powders to form a slurry with a certain viscosity, and then perform a degassing treatment; Step 3: Pour the degassed slurry into the mold, then seal the injection port, flip the lower side of the mold to the upper side, flip it 3-8 times, and perform vacuum debinding in a vacuum degreasing furnace to obtain a green body; Step 4: calcining and sintering the obtained green body to obtain the desired transparent alumina ceramic substrate.

[0019] The transparent alumina ceramic raw materials of this embodiment are as follows: 90-92 parts of alumina raw material, 3-10 parts of sintering aid, 3-5 parts of plasticizer, 2-3 parts of solvent, 1-2 parts of defoaming agent.

[0020] The alumina raw material of this embodiment includes alumina powder and magnesium oxide powder, and the mass ratio of the alumina powder to the magnesium oxide powder is (90-95):1.

[0021] The sintering aid of this embodiment is a mixture of one or more of silicon dioxide, lithium carbonate, yttrium oxide, and cesium oxide, and the plasticizer is a mixture of one or more of polyethylene glycol, phthalate, and tolyl butyl phthalate.

[0022] The solvent of this embodiment is a mixture of anhydrous ethanol and isopropanol, the mass ratio of anhydrous ethanol to isopropanol is 3:7, and the defoaming agent is one of tributyl phosphate or silicone oil.

[0023] When the slurry in step 2 of this embodiment is poured into the mold, the slurry is stirred slowly at a stirring speed of 70-80 r / min.

[0024] The mold in step 2 of this embodiment is kept for 2-3 minutes after being flipped, and the interval between each flipping is 5-10 minutes.

[0025] In step 2 of this embodiment, the heating rate during the debinding process is 50-60°C / h, and the temperature is raised to 200-300°C and kept for 0.5-1h, so that the slurry is dried in a high temperature environment to ensure that the solvent evaporates slowly. After preliminary drying, the hardness of the slurry increases to form a green body.

[0026] During sintering of this embodiment, the green body is placed in a graphite crucible, placed in a sintering furnace with flowing nitrogen, the stable pressure is within 20-40KPa, the temperature is increased to 1400°C at a heating rate of 8-12°C / min, then the temperature is increased to 1600°C at a heating rate of 6-8°C / min, and after keeping the temperature for 2-3 hours, the temperature is reduced to 1100°C at a cooling rate of 1-2°C / min, and then self-cooled to room temperature under flowing nitrogen to obtain a finished substrate.

[0027] This embodiment also includes polishing and grinding the transparent alumina ceramic substrate to make its smoothness Ra less than 0.2 mm.

[0028] Example 1. The present invention of this embodiment provides a method for preparing a transparent alumina ceramic substrate, comprising the following steps: Step 1: prepare transparent alumina ceramic raw materials, pour the prepared raw materials into a grinding device, start the grinding device to perform multi-stage grinding and crushing treatment on the raw materials to obtain raw material powder; Step 2: Mix the obtained raw material powders evenly, filter through a 50-mesh sieve, and use a stirring device to stir the powders to form a slurry with a certain viscosity, and then perform a degassing treatment; Step 3: Pour the degassed slurry into the mold, then seal the injection port, flip the mold from the bottom to the top, flip it 3 times, and perform vacuum debinding in a vacuum degreasing furnace to obtain a green body; Step 4: calcining and sintering the obtained green body to obtain the desired transparent alumina ceramic substrate.

[0029] The transparent alumina ceramic raw materials of this embodiment are as follows: 90 parts of alumina raw material, 3 parts of sintering aid, 3 parts of plasticizer, 2 parts of solvent, and 1 part of defoaming agent.

[0030] The alumina raw material of this embodiment includes alumina powder and magnesium oxide powder, and the mass ratio of the alumina powder to the magnesium oxide powder is 90:1.

[0031] The sintering aid of this embodiment is a mixture of one or more of silicon dioxide, lithium carbonate, yttrium oxide, and cesium oxide, and the plasticizer is a mixture of one or more of polyethylene glycol, phthalate, and tolyl butyl phthalate.

[0032] The solvent of this embodiment is a mixture of anhydrous ethanol and isopropanol, the mass ratio of anhydrous ethanol to isopropanol is 3:7, and the defoaming agent is one of tributyl phosphate or silicone oil.

[0033] When the slurry in step 2 of this embodiment is poured into the mold, the slurry is stirred slowly at a stirring speed of 70 r / min.

[0034] The mold in step 2 of this embodiment is kept for 2-3 minutes after being turned over, and the interval between each turning is 5 minutes.

[0035] In step 2 of this embodiment, the heating rate during the debinding process is 50°C / h, and the temperature is raised to 200°C and kept for 0.5h, so that the slurry is dried in a high temperature environment to ensure that the solvent evaporates slowly. After preliminary drying, the hardness of the slurry increases to form a green body.

[0036] During sintering of this embodiment, the green body is placed in a graphite crucible, placed in a sintering furnace with flowing nitrogen, the stable pressure is within 20KPa, the temperature is increased to 1400°C at a heating rate of 8°C / min, then the temperature is increased to 1600°C at a heating rate of 6°C / min, after being kept warm for 2h, the temperature is lowered to 1100°C at a cooling rate of 1°C / min, and then self-cooled to room temperature under flowing nitrogen to obtain a finished substrate.

[0037] This embodiment also includes polishing and grinding the transparent alumina ceramic substrate to make its smoothness Ra less than 0.2 mm.

[0038] Example 2. The present invention of this embodiment provides a method for preparing a transparent alumina ceramic substrate, comprising the following steps: Step 1: prepare transparent alumina ceramic raw materials, pour the prepared raw materials into a grinding device, start the grinding device to perform multi-stage grinding and crushing treatment on the raw materials to obtain raw material powder; Step 2: Mix the obtained raw material powders evenly, filter through a 55-mesh sieve, and use a stirring device to stir the powders to form a slurry with a certain viscosity, and then perform a degassing treatment; Step 3: Pour the degassed slurry into the mold, then seal the injection port, flip the mold from the bottom to the top, flip it 5 times, and perform vacuum debinding in a vacuum degreasing furnace to obtain a green body; Step 4: calcining and sintering the obtained green body to obtain the desired transparent alumina ceramic substrate.

[0039] The transparent alumina ceramic raw materials of this embodiment are as follows: 91 parts of alumina raw material, 8 parts of sintering aid, 4 parts of plasticizer, 3 parts of solvent, and 1 part of defoaming agent.

[0040] The alumina raw material of this embodiment includes alumina powder and magnesium oxide powder, and the mass ratio of alumina powder to magnesium oxide powder is (92:1).

[0041] The sintering aid of this embodiment is a mixture of one or more of silicon dioxide, lithium carbonate, yttrium oxide, and cesium oxide, and the plasticizer is a mixture of one or more of polyethylene glycol, phthalate, and tolyl butyl phthalate.

[0042] The solvent of this embodiment is a mixture of anhydrous ethanol and isopropanol, the mass ratio of anhydrous ethanol to isopropanol is 3:7, and the defoaming agent is one of tributyl phosphate or silicone oil.

[0043] When the slurry in step 2 of this embodiment is poured into the mold, the slurry is stirred slowly at a stirring speed of 75 r / min.

[0044] The mold in step 2 of this embodiment is kept for 3 minutes after being turned over, and the interval between each turning is 8 minutes.

[0045] In step 2 of this embodiment, the heating rate during the debinding process is 55°C / h, and the temperature is raised to 250°C and kept for 0.8h, so that the slurry is dried in a high temperature environment to ensure that the solvent evaporates slowly. After preliminary drying, the hardness of the slurry increases to form a green body.

[0046] During sintering of this embodiment, the green body is placed in a graphite crucible, placed in a sintering furnace with flowing nitrogen, the stable pressure is within 30KPa, the temperature is increased to 1400°C at a heating rate of 10°C / min, then the temperature is increased to 1600°C at a heating rate of 7°C / min, after being kept warm for 2.5 hours, the temperature is lowered to 1100°C at a cooling rate of 1°C / min, and then self-cooled to room temperature under flowing nitrogen to obtain a finished substrate.

[0047] This embodiment also includes polishing and grinding the transparent alumina ceramic substrate to make its smoothness Ra less than 0.2 mm.

[0048] Example 3. The present invention of this embodiment provides a method for preparing a transparent alumina ceramic substrate, comprising the following steps: Step 1: prepare transparent alumina ceramic raw materials, pour the prepared raw materials into a grinding device, start the grinding device to perform multi-stage grinding and crushing treatment on the raw materials to obtain raw material powder; Step 2: Mix the obtained raw material powders evenly, filter through a 60-mesh sieve, and use a stirring device to stir the powders to form a slurry with a certain viscosity, and then perform a degassing treatment; Step 3: Pour the degassed slurry into the mold, then seal the injection port, flip the mold from the bottom to the top, flip it 8 times, and perform vacuum debinding in a vacuum degreasing furnace to obtain a green body; Step 4: calcining and sintering the obtained green body to obtain the desired transparent alumina ceramic substrate.

[0049] The transparent alumina ceramic raw materials of this embodiment are as follows: 92 parts of alumina raw material, 10 parts of sintering aid, 5 parts of plasticizer, 3 parts of solvent, and 2 parts of defoaming agent.

[0050] The alumina raw material of this embodiment includes alumina powder and magnesium oxide powder, and the mass ratio of the alumina powder to the magnesium oxide powder is 95:1.

[0051] The sintering aid of this embodiment is a mixture of one or more of silicon dioxide, lithium carbonate, yttrium oxide, and cesium oxide, and the plasticizer is a mixture of one or more of polyethylene glycol, phthalate, and tolyl butyl phthalate.

[0052] The solvent of this embodiment is a mixture of anhydrous ethanol and isopropanol, the mass ratio of anhydrous ethanol to isopropanol is 3:7, and the defoaming agent is one of tributyl phosphate or silicone oil.

[0053] When the slurry in step 2 of this embodiment is poured into the mold, the slurry is stirred slowly at a stirring speed of 80 r / min.

[0054] The mold in step 2 of this embodiment is kept for 3 minutes after being flipped, and the interval between each flipping is 5-10 minutes.

[0055] In step 2 of this embodiment, the heating rate during the debinding process is 60°C / h, and the temperature is raised to 300°C and kept for 1 hour, so that the slurry is dried in a high temperature environment to ensure that the solvent evaporates slowly. After preliminary drying, the hardness of the slurry increases to form a green body.

[0056] During sintering of this embodiment, the green body is placed in a graphite crucible, placed in a sintering furnace with flowing nitrogen, the stable pressure is within 40KPa, the temperature is increased to 1400°C at a heating rate of 12°C / min, and then the temperature is increased to 1600°C at a heating rate of 8°C / min. After keeping the temperature for 3 hours, the temperature is lowered to 1100°C at a cooling rate of 2°C / min, and then self-cooled to room temperature under flowing nitrogen to obtain a finished substrate.

[0057] This embodiment also includes polishing and grinding the transparent alumina ceramic substrate to make its smoothness Ra less than 0.2 mm.

[0058] Comparative Example 1. The difference from Example 3 is that a common method is used to prepare the transparent alumina ceramic substrate.

[0059] The products of Examples 1-3 and Comparative Example 1 were subjected to performance tests; Four transparent alumina ceramic substrate samples were prepared, with one sample in each group divided into four groups in total. Each group corresponded to Examples 1-3 and Comparative Example 1 and was numbered A / B / C / D. Finally, the density, thermal conductivity, transmittance and upper and lower layer density ratio of the transparent alumina ceramic substrates in groups A / B / C / D were tested respectively. The test results are shown in the following table.

[0060] It can be seen from Examples 1-3 that the transparent alumina ceramic substrate made using the present invention adopts high-purity nano-alumina as a raw material and doped with magnesium oxide to inhibit the rapid growth of ceramic grains at high temperatures. The obtained transparent alumina ceramic sample has a smaller grain size, a higher density, better light transmittance, and a more uniform density, thereby improving the production quality of the alumina ceramic substrate.

[0061] In addition, it was found from Examples 1-3 and Comparative Example 1 that a powder slurry with uniform particle size was obtained by grinding and screening the transparent alumina ceramic raw material. The slurry was kept slowly stirred when poured into the mold. The prefabricated slurry was dried and debinded to obtain an intermediate embryo. The embryo was then turned upside down to solidify, so that it had a certain degree of coagulation, thereby avoiding precipitation of materials with high specific gravity during the solidification process of the slurry.

[0062] The innovation of the present invention is: The present invention grinds and screens transparent alumina ceramic raw materials to obtain a powder slurry with uniform particle size, keeps the slurry slowly stirred when pouring it into a mold, obtains an intermediate embryo through drying and debinding the prefabricated slurry, and then turns the embryo upside down to solidify it, so that it has a certain degree of coagulation, avoids precipitation of materials with high specific gravity during the solidification process of the slurry, makes the density difference of the finally obtained ceramic substrate small, the density is more uniform, and the production quality of the alumina ceramic substrate is improved. By using high-purity nano-alumina as a raw material and doping magnesium oxide to inhibit the rapid growth of ceramic grains at high temperature, the obtained transparent alumina ceramic sample has a smaller grain size, so that it has a large density and better light transmittance. At the same time, the introduction of a sintering aid can reduce the sintering temperature of the high-purity alumina ceramic, which not only reduces energy consumption but also improves sintering shrinkage and controllability. The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which shall fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a transparent alumina ceramic substrate, characterized in that: The steps include: Step 1: prepare transparent alumina ceramic raw materials, pour the prepared raw materials into a grinding device, start the grinding device to perform multi-stage grinding and crushing treatment on the raw materials to obtain raw material powder; Step 2: Mix the obtained raw material powders evenly, filter through a 50-60 mesh sieve, and use a stirring device to stir the powders to form a slurry with a certain viscosity, and then perform a degassing treatment; Step 3: Pour the degassed slurry into the mold, then seal the injection port, flip the bottom side of the mold to the top side, flip 3-8 times, and perform vacuum debinding in a vacuum degreasing furnace to obtain a green body; Step 4: calcining and sintering the obtained green body to obtain the desired transparent alumina ceramic substrate.

2. The method for preparing a transparent alumina ceramic substrate according to claim 1, characterized in that: The transparent alumina ceramic raw materials are as follows: 90-92 parts of alumina raw material, 3-10 parts of sintering aid, 3-5 parts of plasticizer, 2-3 parts of solvent, 1-2 parts of defoaming agent.

3. The method for preparing a transparent alumina ceramic substrate according to claim 2, characterized in that: The alumina raw material includes alumina powder and magnesium oxide powder, and the mass ratio of the alumina powder to the magnesium oxide powder is (90-95):

1.

4. The method for preparing a transparent alumina ceramic substrate according to claim 3, characterized in that: The sintering aid is a mixture of one or more of silicon dioxide, lithium carbonate, yttrium oxide, and cesium oxide; the plasticizer is a mixture of one or more of polyethylene glycol, phthalate, and tolyl butyl phthalate.

5. The method for preparing a transparent alumina ceramic substrate according to claim 4, characterized in that: The solvent is a mixture of anhydrous ethanol and isopropanol, the mass ratio of the anhydrous ethanol to the isopropanol is 3:7, and the defoaming agent is one of tributyl phosphate or silicone oil.

6. The method for preparing a transparent alumina ceramic substrate according to claim 1, characterized in that: When the slurry in step 2 is poured into the mold, the slurry is stirred slowly at a stirring speed of 70-80 r / min.

7. The method for preparing a transparent alumina ceramic substrate according to claim 6, characterized in that: The mold in step 2 is kept for 2-3 minutes after being flipped, and the interval between each flipping is 5-10 minutes.

8. The method for preparing a transparent alumina ceramic substrate according to claim 7, characterized in that: The heating rate in the debinding process in step 2 is 50-60°C / h, and the temperature is raised to 200-300°C and kept for 0.5-1h, so that the slurry is dried in a high temperature environment to ensure that the solvent evaporates slowly. After preliminary drying, the hardness of the slurry increases to form a green body.

9. The method for preparing a transparent alumina ceramic substrate according to claim 1, characterized in that: During the sintering, the green body is placed in a graphite crucible, placed in a sintering furnace with flowing nitrogen, the stable pressure is within 20-40KPa, the temperature is increased to 1400°C at a heating rate of 8-12°C / min, then the temperature is increased to 1600°C at a heating rate of 6-8°C / min, after keeping the temperature for 2-3 hours, the temperature is reduced to 1100°C at a cooling rate of 1-2°C / min, and then self-cooled to room temperature under flowing nitrogen to obtain a finished substrate.

10. The method for preparing a transparent alumina ceramic substrate according to claim 9, characterized in that: The method also includes polishing and grinding the transparent alumina ceramic substrate to make its smoothness Ra less than 0.2 mm.

Citation Information

Patent Citations

  • BE462063A

  • Preparation method of transparent alumina ceramic