Co-doped barium titanate ceramic dielectric material as well as preparation method and application thereof

By using 80-140nm BaTiO3 particles and doping materials in barium titanate ceramic dielectric materials for prefiring and ball milling, grain growth is controlled, and a co-doped material with an average particle size of 160-230nm was prepared, and the solution is solved The problem of large fluctuation in the dielectric constant of barium titanate ceramic dielectric materials at high temperatures has achieved optimization of dielectric temperature stability and capacitance change rate, meeting the requirements of X7R.

CN118930251APending Publication Date: 2024-11-12SHENZHEN INST OF ADVANCED ELECTRONICS MATERIALS

Patent Information

Application Number
CN202411077192.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing barium titanate ceramic dielectric materials have excessive grain size growth during sintering, resulting in large fluctuations in the dielectric material's dielectric constant, limiting its application range at high temperatures, and increasing the number of stacks to obtain large-capacity capacitors. Will reduce reliability.

Method used

BaTiO3 particles of 80-140nm are used as the main material, and doped materials such as MgO, SiO2, MnO2 and Ho2O3 are added, and pre-sintered and wet ball milling are performed to control grain growth, and a total of 160-230nm is prepared. Doped with barium titanate ceramic dielectric material inhibits grain growth and achieves a flat dielectric curve.

Benefits of technology

The dielectric temperature stability of ceramic capacitors is improved, and the capacitance change rate is between -15% and 15%, which meets the requirements of X7R, and improves the reliability and performance stability of multi-layer ceramic capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930251A_ABST
    Figure CN118930251A_ABST
Patent Text Reader

Abstract

The invention relates to a co-doped barium titanate ceramic dielectric material, the co-doped barium titanate ceramic dielectric material comprises a main body material and a doping material, the main body material comprises BaTiO3 particles, the average particle size of the BaTiO3 particles is 80-140 nm, and the doping material comprises MgO, SiO2, MnO2 and Ho2O3. BaTiO3 is used as a main body material, so that the process complexity can be reduced, and the cost can be saved. According to the invention, the average particle size of the main body BaTiO3 particles is 80-140nm, and the doping material is added, so that the crystal grain growth easily occurring in the sintering process can be effectively inhibited, and finally, the ceramic dielectric material with the average particle size of 160-230nm can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ceramic dielectrics, and in particular to a co-doped barium titanate ceramic dielectric material and a preparation method and application thereof. Background Art

[0002] Multilayer ceramic capacitors (MLCCs) are widely used in communication infrastructure equipment circuits in the fields of communication equipment, automotive electronics, industrial machinery, medical equipment, etc. They can be used as power bypass capacitors, such as liquid crystal modules (liquid crystal drive voltage lines), high power supply voltage LSI / IC / OP amplifiers, or as smoothing capacitors, such as DC-DC converters (input and output), switching power supplies (secondary side), etc.

[0003] In recent years, with the development of the 5G era, the miniaturization of mobile electronic devices has made MLCC gradually develop in the direction of miniaturization and large capacity. Barium titanate (BaTiO3) is the base material of Class II capacitors in MLCC, which has a high dielectric constant. However, its dielectric constant fluctuates greatly at -90°C, 0°C and 125°C, which also limits the application range of barium titanate. The dielectric material temperature coefficients of Class II capacitors include X5R, X6R, X7R, etc. The capacitor specification of the American Electronics Industry Association (EIA) mentions that when the temperature of X7R is between -55°C and 125°C, the capacitance change rate must be between -15% and 15%.

[0004] However, in order to obtain a large-capacity barium titanate-based MLCC, the number of stacking layers needs to be increased, which leads to a significant decrease in the reliability of the MLCC. In order to increase its reliability and ensure the performance stability of the MLCC, a single-layer dielectric layer must have a thickness of 4 to 6 grains, so the grain size of a single-layer dielectric layer in the MLCC is preferably controlled below 230nm. Therefore, it is crucial to study barium titanate raw material powders with smaller particle sizes and methods to limit the growth of its grain size during the sintering process.

[0005] Therefore, how to achieve a smaller average particle size of the co-doped barium titanate ceramic dielectric material so as to reduce the dielectric thickness of the prepared multilayer ceramic capacitor has become a problem that needs to be solved urgently. Summary of the invention

[0006] In order to solve the above technical problems, the purpose of the present invention is to design a co-doped barium titanate ceramic dielectric material with a small average particle size prepared by using small-particle barium titanate as a raw material, and at the same time use doping materials to control the dielectric constant and inhibit grain growth during the subsequent sintering process, thereby obtaining a co-doped barium titanate ceramic dielectric material with a small-particle barium titanate dielectric layer and a flat dielectric curve.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a co-doped barium titanate ceramic dielectric material, wherein the raw materials for preparing the co-doped barium titanate ceramic dielectric material include a main material and a doping material; the main material includes BaTiO3 particles, and the average particle size of the BaTiO3 particles is 80-140nm, for example, it can be 80nm, 85nm, 90nm, 95nm, 100nm, 105nm, 110nm, 115nm, 120nm, 125nm, 130nm, 135nm or 140nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; the doping material includes MgO, SiO2, MnO2 and Ho2O3.

[0009] The present invention uses BaTiO3 as the main material, which can reduce the complexity of the process and save costs. According to traditional experience, after BaTiO3 nanoparticles are sintered to form a multilayer ceramic capacitor (MLCC), the average grain size grows by 20%-35%, while small-sized barium titanate particles have higher activity and higher specific surface energy, and the average grain size grows more after sintering. Therefore, the present invention controls the average particle size of the main BaTiO3 particles to be 80-140nm, and suppresses the grain growth during the sintering process by adding doping materials, and finally obtains a ceramic dielectric material with an average particle size of 160-230nm.

[0010] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0011] Preferably, based on the total molar amount of the co-doped barium titanate ceramic dielectric material as 100%, the added amount of the main material is 90.0-92.0 mol%, for example, it can be 90.0 mol%, 90.1 mol%, 90.2 mol%, 90.3 mol%, 90.4 mol%, 90.5 mol%, 90.6 mol%, 90.7 mol%, 90.8 mol%, 90.9 mol%, 91.0 mol%, 91.1 mol%, 91.2 mol%, 91.3 mol%, 91.4 mol%, 91.5 mol%, 91.6 mol%, 91.7 mol%, 91.8 mol%, 91.9 mol% or 92.0 mol%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0012] Taking the total molar amount of the co-doped barium titanate ceramic dielectric material as 100%, the total added amount of the doping material is 8.0-10.0 mol%, for example, it can be 8.0 mol%, 8.1 mol%, 8.2 mol%, 8.3 mol%, 8.4 mol%, 8.5 mol%, 8.6 mol%, 8.7 mol%, 8.8 mol%, 8.9 mol%, 9.0 mol%, 9.1 mol%, 9.2 mol%, 9.3 mol%, 9.4 mol%, 9.5 mol%, 9.6 mol%, 9.7 mol%, 9.8 mol%, 9.9 mol% or 10 mol%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0013] Preferably, based on the total molar amount of the co-doped barium titanate ceramic dielectric material as 100%, the added amount of MgO is 3.0-4.0 mol%, for example, it can be 3.0 mol%, 3.1 mol%, 3.2 mol%, 3.3 mol%, 3.4 mol%, 3.5 mol%, 3.6 mol%, 3.7 mol%, 3.8 mol%, 3.9 mol% or 4.0 mol%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 3.5-4 mol%.

[0014] Preferably, based on the total molar amount of the co-doped barium titanate ceramic dielectric material as 100%, the added amount of SiO2 is 1.0-2.0 mol%, for example, it can be 1.0 mol%, 1.1 mol%, 1.2 mol%, 1.3 mol%, 1.4 mol%, 1.5 mol%, 1.6 mol%, 1.7 mol%, 1.8 mol%, 1.9 mol% or 2.0 mol%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 1.5-2 mol%.

[0015] Preferably, based on the total molar amount of the co-doped barium titanate ceramic dielectric material as 100%, the added amount of MnO2 is 1.0-2.0 mol%, for example, it can be 1.0 mol%, 1.1 mol%, 1.2 mol%, 1.3 mol%, 1.4 mol%, 1.5 mol%, 1.6 mol%, 1.7 mol%, 1.8 mol%, 1.9 mol% or 2.0 mol%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 1.5-2.0 mol%.

[0016] Preferably, based on the total molar amount of the co-doped barium titanate ceramic dielectric material as 100%, the added amount of Ho2O3 is 1.0-2.0 mol%, for example, it can be 1.0 mol%, 1.1 mol%, 1.2 mol%, 1.3 mol%, 1.4 mol%, 1.5 mol%, 1.6 mol%, 1.7 mol%, 1.8 mol%, 1.9 mol% or 2.0 mol%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 1.0-1.5 mol%.

[0017] The present invention further optimizes the molar content of each doping material, wherein Ho 3+ Substituting Ba in BaTiO3(ABO3) system 2+ , donor doping into the A site, Mn 4+ Replace Ti 4+ , acceptor doping is performed at the B site to generate oxygen vacancies. On the one hand, barium vacancies and oxygen vacancies move to the grain boundaries, causing a pinning effect, hindering the movement of grain boundaries and inhibiting the growth of grains. Among them, Ho2O3 can regulate the dielectric constant, so in Si 4+ Mg 2+ and Mn 4+ With the synergistic effect of the three, a co-doped barium titanate ceramic dielectric material with a more dense, uniform structure and a flatter dielectric curve can be prepared, so that the prepared ceramic capacitor has good dielectric temperature stability.

[0018] Preferably, the average particle size of the co-doped barium titanate ceramic dielectric material is 160-230 nm, for example, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, 210 nm, 220 nm or 230 nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] In a second aspect, the present invention provides a method for preparing the co-doped barium titanate ceramic dielectric material as described in the first aspect, the preparation method comprising:

[0020] The main material and MgO are mixed and wet ball-milled, dried, and then pre-calcined to obtain a pre-prepared powder;

[0021] The prepared powder is mixed with other doping materials and wet-milled, and then dried to obtain the co-doped barium titanate ceramic dielectric material.

[0022] The pre-sintering treatment in the present invention enables the doping material to be preferentially coated on the surface of the main phase material, and the subsequent doping material forms a double-layer shell structure, thereby achieving the effect of controlling the growth of small grains and good temperature stability. Compared with the traditional process of directly mixing the main material and all the doping materials together without pre-sintering treatment, the barium titanate ceramic dielectric material prepared by the present invention successfully controls the particle size growth and obtains a flat dielectric curve.

[0023] Preferably, the temperature of the pre-firing treatment is 900-1100°C, for example, it can be 910°C, 920°C, 930°C, 940°C, 950°C, 960°C, 970°C, 980°C, 990°C, 1000°C or 1100°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] Preferably, the preparation method of the co-doped barium titanate ceramic dielectric material specifically includes: mixing a BaTiO3 main material with an average particle size of 80-140nm and MgO in proportion, using zirconium oxide balls as ball milling media, ethanol as ball milling medium liquid, wet ball milling for 24 hours, grinding after drying, pre-sintering in air at 900-1100°C, and keeping warm for 2-3 hours to obtain a preliminary powder; then mixing the preliminary powder with the doping material in proportion, using zirconium oxide balls as ball milling media, wet ball milling for 24 hours, and drying to obtain a co-doped barium titanate ceramic dielectric material with an average particle size of 160-230nm.

[0025] The present invention prepares a doped barium titanate ceramic dielectric material with a small particle size and a flat dielectric curve by first doping Mg to control grain growth and then doping the remaining materials. Among them, SiO2 is added as a sintering aid to reduce and widen the sintering temperature to prevent the grain growth of ceramic particles during the sintering process. MgO is added to refine the grains. Mg tends to stay at the grain boundary after sintering in barium titanate, thereby controlling the growth of grains, obtaining a suitable grain size, and promoting the mass transfer process of BaTiO3 to improve the density of ceramics; and the combination of SiO2 and MgO will produce a liquid phase during the ceramic sintering process. The liquid phase uniformly wraps each particle to prevent the particles from growing excessively. At the same time, the addition of MnO2 can further inhibit the growth of grains, so that the obtained barium titanate ceramic dielectric material has a smaller average particle size. In addition, the liquid phase on the surface of the inner electrode can hinder the diffusion of metal elements into the dielectric layer, enhance the reliability of MLCC, and increase the excellence of the present invention in the application field of MLCC.

[0026] In a third aspect, the present invention provides a multilayer ceramic capacitor prepared from the co-doped barium titanate ceramic dielectric material as described in the first aspect.

[0027] The MLCC prepared by the present invention has higher dielectric temperature stability, can have a smaller capacitance change rate within a wide temperature range, and meets the X7R requirements of EIA.

[0028] Preferably, the dielectric constant of the multilayer ceramic capacitor at 25° C. is 1400-1800, for example, 1400, 1450, 1500, 1550, 1600, 1650, 1700, 1750 or 1800, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] Preferably, the capacitance change rate of the multilayer ceramic capacitor is between -15% and 15% at -55°C to 125°C, meeting the X7R requirement of EIA.

[0030] In a fourth aspect, the present invention provides a method for preparing a multilayer ceramic capacitor as described in the third aspect, the preparation method comprising:

[0031] The co-doped barium titanate ceramic dielectric material as described in the first aspect is sintered in a reducing atmosphere to obtain the multilayer ceramic capacitor.

[0032] The multilayer ceramic capacitor provided by the present invention has a simple preparation process, does not contain toxic substances, is well matched with base metal inner electrodes such as nickel, has a dense ceramic body, small grains, few defects, and has broad application prospects.

[0033] Preferably, the sintering temperature is 1150°C-1250°C, for example, it can be 1150°C, 1160°C, 1170°C, 1180°C, 1190°C, 1200°C, 1210°C, 1220°C, 1230°C, 1240°C or 1250°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the preparation method of the multilayer ceramic capacitor specifically includes: the obtained co-doped barium titanate ceramic dielectric material powder is made into a slurry, cast into a 0.8-1.5μm diaphragm, and then subjected to electrode printing, lamination, pressing, and cutting to form a green body with a certain shape and size. Among them, nickel paste is used as the inner electrode, and the number of layers is 60. The green sheet is sintered for 2-4h at 1150℃-1250℃ in a reducing atmosphere (1% H2+99% N2), and then the temperature is reduced to 25℃ to complete the sintering to form a monolithic structure porcelain body. Subsequently, copper paste is applied to both ends of the monolithic structure porcelain body by copper dipping, and then sintered to form a copper electrode firmly bonded to the porcelain body, and then a nickel layer is electroplated on the surface of the copper electrode, and a tin layer is electroplated for the second time to obtain an MLCC sample.

[0035] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0036] Compared with the prior art, the present invention has at least the following beneficial effects:

[0037] (1) The present invention uses BaTiO3 particles with an average particle size of 80-140nm as the main material and dopes materials including MgO, SiO2, MnO2 and Ho2O3 to prepare a doped barium titanate ceramic dielectric material having a small particle size barium titanate dielectric layer and a flat dielectric curve, wherein Ho2O3 can regulate the dielectric constant. 4+ Mg 2+ and Mn 4+ With the synergistic effect of the three, a co-doped barium titanate ceramic dielectric material with a more dense, uniform structure and a flatter dielectric curve can be prepared.

[0038] (2) The multilayer ceramic capacitor MLCC prepared by sintering the doped barium titanate ceramic dielectric material in a reducing atmosphere has a dielectric constant between 1400 and 1800 and can meet the X7R temperature characteristic requirements, that is, the capacitance change rate is between -15% and 15% at a temperature of -55°C to 125°C. The doped barium titanate ceramic dielectric material and multilayer ceramic capacitor provided by the present invention have a simple preparation process, do not contain toxic substances, have good matching with base metal internal electrodes such as nickel, have a dense ceramic body, small grains, few defects, and have broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 is a transmission electron microscope image of the MLCC sample in Application Example 1 of the present invention;

[0040] Figure 2 is a transmission electron microscope image of the MLCC sample in comparative application example 1 of the present invention;

[0041] Figure 3 is a grain size distribution diagram of the MLCC sample in Application Example 1 of the present invention;

[0042] Figure 4 is a grain size distribution diagram of the MLCC sample in comparative application example 1 of the present invention;

[0043] Figure 5 It is a schematic diagram comparing the dielectric constant and temperature of the MLCC samples of Application Example 1 of the present invention and Comparative Application Example 1;

[0044] Figure 6 It is a schematic diagram comparing the capacitance change rate and temperature of the MLCC samples of Application Example 1 of the present invention and Comparative Application Example 1; DETAILED DESCRIPTION

[0045] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0046] In the following examples, unless otherwise specified, all reagents and consumables were purchased from conventional reagent manufacturers in the field; unless otherwise specified, the experimental methods and technical means used were conventional methods and means in the field.

[0047] Example 1

[0048] The present embodiment provides a co-doped barium titanate ceramic dielectric material, wherein the co-doped barium titanate ceramic dielectric material includes 91 mol % BaTiO 3 particles with an average particle size of 120 nm, 4 mol % MgO, 2 mol % SiO 2 , 1.0 mol % MnO 2 and 2.0 mol % Ho 2 O 3 .

[0049] The co-doped barium titanate ceramic dielectric material provided in this embodiment specifically includes the following steps:

[0050] The main material BaTiO3 with an average particle size of 120nm and MgO are mixed in proportion, zirconium oxide balls are used as ball milling media, ethanol is used as ball milling medium liquid, wet ball milling is carried out for 24 hours, and then dried and ground. The temperature is raised to 1000°C in air for pre-sintering treatment, and the temperature is kept for 3 hours to obtain a preliminary powder; the preliminary powder is then mixed with other doping materials in proportion, zirconium oxide balls are used as ball milling media, wet ball milling is carried out for 24 hours, and co-doped barium titanate ceramic dielectric material is obtained after drying.

[0051] Example 2

[0052] The present embodiment provides a co-doped barium titanate ceramic dielectric material, wherein the co-doped barium titanate ceramic dielectric material includes 92 mol % BaTiO 3 particles with an average particle size of 100 nm, 3.5 mol % MgO, 1.5 mol % SiO 2 , 1.0 mol % MnO 2 and 2.0 mol % Ho 2 O 3 .

[0053] The co-doped barium titanate ceramic dielectric material provided in this embodiment specifically includes the following steps:

[0054] The main material BaTiO3 with an average particle size of 100nm and MgO are mixed in proportion, zirconium oxide balls are used as ball milling media, ethanol is used as ball milling medium liquid, wet ball milling is carried out for 24 hours, and then dried and ground. The mixture is pre-sintered at 900°C in air and kept warm for 2 hours to obtain a preliminary powder. The preliminary powder is then mixed with other doping materials in proportion, zirconium oxide balls are used as ball milling media, wet ball milling is carried out for 24 hours, and the co-doped barium titanate ceramic dielectric material is obtained after drying.

[0055] Comparative Example 1

[0056] This comparative example provides a co-doped barium titanate ceramic dielectric material, which differs from Example 1 in that no step-by-step treatment and pre-sintering treatment are used. BaTiO3 main material with an average particle size of 120 nm and MgO, SiO2, MnO2, and Ho2O3 are mixed and ball-milled at the same molar ratio as in Example 1, zirconium oxide balls are used as ball-milling media, and ethanol is used as ball-milling medium liquid, and wet ball-milling is performed for 24 hours, and the co-doped barium titanate ceramic dielectric material is obtained after drying.

[0057] Comparative Example 2

[0058] This comparative example provides a co-doped barium titanate ceramic dielectric material and a multilayer ceramic capacitor, which differs from Example 1 only in that MgO is not added to the raw materials for preparing the co-doped barium titanate ceramic dielectric material, and the reduced molar amount is proportionally distributed to the remaining doping materials.

[0059] Comparative Example 3

[0060] This comparative example provides a co-doped barium titanate ceramic dielectric material and a multilayer ceramic capacitor, which differs from Example 1 only in that no MnO2 is added to the raw materials for preparing the co-doped barium titanate ceramic dielectric material, and the reduced molar amount is proportionally distributed to the remaining doping materials.

[0061] Comparative Example 4

[0062] This comparative example provides a co-doped barium titanate ceramic dielectric material and a multilayer ceramic capacitor, which differs from Example 1 only in that SiO2 is not added to the raw materials for preparing the co-doped barium titanate ceramic dielectric material, and the reduced molar amount is proportionally distributed to the remaining doping materials.

[0063] Comparative Example 5

[0064] This comparative example provides a co-doped barium titanate ceramic dielectric material, which is different from Example 1 only in that the co-doped barium titanate ceramic dielectric material is replaced with 91 mol % of BaTiO 3 particles with an average particle size of 150 nm.

[0065] Application Example 1

[0066] This application example provides a multilayer ceramic capacitor, and the multilayer ceramic capacitor specifically includes the following steps:

[0067] The co-doped barium titanate ceramic dielectric material powder obtained in Example 1 is made into a slurry, cast into a 1.2μm diaphragm, and then subjected to electrode printing, lamination, pressing, and cutting to form a green body with a certain shape and size. Among them, nickel paste is used as the internal electrode, and the number of laminations is 60. The green sheet is sintered for 2 hours at 1200°C in a reducing atmosphere (1% H2+99% N2), and then the temperature is reduced to 25°C to complete the sintering to form a monolithic structure porcelain body. Subsequently, copper paste is applied to both ends of the monolithic structure porcelain body by copper dipping, and then sintered to form a copper electrode firmly bonded to the porcelain body, and then a nickel layer is electroplated on the surface of the copper electrode, and a tin layer is electroplated for the second time to obtain an MLCC sample.

[0068] The scanning electron microscopy results of the prepared MLCC are as follows: Figure 1 As shown, it can be seen that the MLCC sample has good density and no obvious holes.

[0069] The average particle size distribution of the prepared MLCC is shown in Figure 3 As shown, the ceramic grain size distribution of MLCC can be seen, and the average grain size is about 182nm.

[0070] The relationship between the dielectric constant and temperature of the prepared MLCC is as follows: Figure 5 As shown, it can be seen that MLCC has effectively stabilized the impact of drastic changes in dielectric constant caused by temperature.

[0071] The relationship between the capacitance constant change rate and temperature of the prepared MLCC is as follows: Figure 6 As shown, it can be seen that the capacitance change rate of MLCC is between ±15% when the temperature is between -55℃ and 125℃, which meets the X7R requirement of EIA.

[0072] Application Example 2

[0073] This application example provides a multilayer ceramic capacitor, and the multilayer ceramic capacitor specifically includes the following steps:

[0074] The co-doped barium titanate ceramic dielectric material powder obtained in Example 2 is made into a slurry, cast into a 1μm diaphragm, and then subjected to electrode printing, lamination, pressing, and cutting to form a green body with a certain shape and size. Among them, nickel paste is used as the internal electrode, and the number of laminations is 60. The green sheet is sintered for 2 hours at 1250°C in a reducing atmosphere (1% H2+99% N2), and then the temperature is reduced to 25°C to complete the sintering to form a monolithic structure porcelain body. Subsequently, copper paste is applied to both ends of the monolithic structure porcelain body by copper dipping, and then sintered to form a copper electrode firmly bonded to the porcelain body, and then a nickel layer is electroplated on the surface of the copper electrode, and a tin layer is electroplated for the second time to obtain an MLCC sample.

[0075] Comparative application example 1

[0076] This comparative application example provides a multilayer ceramic capacitor. The preparation method of the multilayer ceramic capacitor differs from the preparation method of Application Example 1 only in that this comparative application example uses the co-doped barium titanate ceramic dielectric material obtained in Comparative Example 1, and the remaining steps are the same as those in Application Example 1.

[0077] The transmission electron microscopy results of the prepared MLCC are as follows: Figure 2 shown.

[0078] The average particle size distribution of the prepared MLCC is shown in Figure 4 As shown, the ceramic grain size distribution of MLCC can be seen, and the average grain size is about 211nm.

[0079] The relationship between the dielectric constant and temperature of the prepared MLCC is as follows: Figure 5 shown.

[0080] The relationship between the capacitance constant change rate and temperature of the prepared MLCC is as follows: Figure 6 As shown, it does not meet the EIA's X7R requirement.

[0081] Comparative Application Example 2

[0082] This comparative application example provides a multilayer ceramic capacitor. The preparation method of the multilayer ceramic capacitor differs from the preparation method of Application Example 1 only in that this comparative application example uses the co-doped barium titanate ceramic dielectric material obtained in Comparative Example 2, and the remaining steps are the same as those in Application Example 1.

[0083] Comparative Application Example 3

[0084] This comparative application example provides a multilayer ceramic capacitor. The preparation method of the multilayer ceramic capacitor differs from the preparation method of Application Example 1 only in that this comparative application example uses the co-doped barium titanate ceramic dielectric material obtained in Comparative Example 3, and the remaining steps are the same as those in Application Example 1.

[0085] Comparative Application Example 4

[0086] This comparative application example provides a multilayer ceramic capacitor. The preparation method of the multilayer ceramic capacitor differs from the preparation method of Application Example 1 only in that this comparative application example uses the co-doped barium titanate ceramic dielectric material obtained in Comparative Example 4, and the remaining steps are the same as those in Application Example 1.

[0087] Comparative Application Example 5

[0088] This comparative application example provides a multilayer ceramic capacitor. The preparation method of the multilayer ceramic capacitor differs from the preparation method of Application Example 1 only in that this comparative application example uses the co-doped barium titanate ceramic dielectric material obtained in Comparative Example 5, and the remaining steps are the same as those in Application Example 1.

[0089] Test method: 1. Use the Thermo Fisher Helios5UX focused ion beam (FIB) to slice the polished ceramic sample to obtain a thin slice sample of about 100nm. Use the JEM-3200FS TEM of Japan Optical Electronics Laboratory for testing.

[0090] 2. The test method for dielectric constant is: use Alpha-A broadband dielectric tester from Novocontrol Technologies of Germany with a 1V driving field, measure the capacitance and loss at different frequencies at a temperature between -60℃ and 200℃, at intervals of 2℃.

[0091] The results are summarized in Table 1.

[0092] Table 1

[0093]

[0094] The test results show that:

[0095] (1) It can be seen from Application Examples 1 and 2 that the present invention controls the average particle size of the main BaTiO3 particles to be 80-140nm, and step-by-step addition of doping materials and pretreatment to inhibit grain growth during sintering, and ultimately a ceramic dielectric material with an average particle size of 160-230nm can be obtained. The material is denser, the particle size distribution is more concentrated, and the dielectric curve is flat, further enabling the prepared ceramic capacitor to have good dielectric temperature stability and meet the EIA's X7R requirements.

[0096] (2) Figure 1 to Figure 6 , as well as the test results of Application Example 1 and Comparative Application Example 1, it can be seen that the present invention can prepare barium titanate ceramic materials with an average particle size of 160-230nm by adding the doping raw materials step by step and pre-firing, and the capacitance change rate is stable between -15% and 15%, and the dielectric loss is smaller, and the technical effect of enhancing the stability of MLCC can be further achieved. When the process is not divided into steps and there is no pre-firing treatment, the dielectric curve is uneven and shows a downward trend, and the technical effect of further reducing the particle size of the barium titanate ceramic dielectric material cannot be achieved, and the reliability performance is reduced, the capacitance change rate exceeds 15%, and the dielectric loss is significantly increased, and the prepared MLCC does not meet the X7R requirements.

[0097] (3) It can be seen from Application Example 1 and Comparative Application Examples 2-4 that the present invention prepares a co-doped barium titanate ceramic dielectric material by doping MgO, SiO2, MnO2 and Ho2O3 materials in barium titanate particles. 4+ Mg 2+ and Mn 4+ The synergistic effect of the three can produce a more dense, uniform and flatter co-doped barium titanate ceramic dielectric material. 3+ Substituting Ba in BaTiO3(ABO3) system 2+ , donor doping into the A site, Mn 4+ Replace Ti 4+ , acceptor doping is carried out at the B site to generate oxygen vacancies. On the one hand, barium vacancies and oxygen vacancies move to the grain boundaries, causing a pinning effect, hindering the movement of grain boundaries, and inhibiting the growth of grains. The average particle size of the prepared co-doped barium titanate ceramic dielectric material is smaller, so that the prepared ceramic capacitor has good dielectric temperature stability.

[0098] (4) It can be seen from Application Example 1 and Comparative Application Example 5 that the present invention can prepare barium titanate ceramic materials with an average particle size of 160-230 nm by controlling the average particle size of the main BaTiO3 particles to 80-140 nm, and further can achieve the technical effect of enhancing the stability of MLCC. However, when the average particle size of the BaTiO3 particles is greater than 140 nm, it is impossible to achieve the technical effect of further reducing the particle size of the barium titanate ceramic dielectric material, and the prepared MLCC does not meet the X7R requirement.

[0099] In summary, the present invention controls the average particle size of the main BaTiO3 particles to 80-140nm, and suppresses the grain growth during the sintering process by adding doping materials, and finally obtains a ceramic dielectric material with an average particle size of 160-230nm, wherein Ho2O3 can regulate the dielectric constant. 4+ Mg 2+ and Mn 4+ The synergistic effect of the three makes the material more dense and uniform and the dielectric curve flat, which further makes the prepared ceramic capacitor have good dielectric temperature stability and meets the EIA's X7R requirements.

[0100] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A co-doped barium titanate ceramic dielectric material, characterized in that: The raw materials for preparing the co-doped barium titanate ceramic dielectric material include a main material and a doping material; The main material includes BaTiO3 particles, and the average particle size of the BaTiO3 particles is 80-140nm; the doping material includes MgO, SiO2, MnO2 and Ho2O3.

2. The co-doped barium titanate ceramic dielectric material according to claim 1, characterized in that: Based on the total molar amount of the co-doped barium titanate ceramic dielectric material being 100%, the added amount of the main material is 90.0-92.0 mol%.

3. The co-doped barium titanate ceramic dielectric material according to claim 1, characterized in that: Based on the total molar amount of the co-doped barium titanate ceramic dielectric material being 100%, the total added amount of the doping material is 8.0-10.0 mol%; Preferably, based on the total molar amount of the co-doped barium titanate ceramic dielectric material as 100%, the added amount of MgO is 3.0-4.0 mol%, preferably 3.5-4.0 mol%; Preferably, based on the total molar amount of the co-doped barium titanate ceramic dielectric material as 100%, the added amount of SiO2 is 1.0-2.0 mol%, preferably 1.5-2.0 mol%; Preferably, based on the total molar amount of the co-doped barium titanate ceramic dielectric material as 100%, the added amount of MnO2 is 1.0-2.0 mol%, preferably 1.5-2.0 mol%; Preferably, based on the total molar amount of the co-doped barium titanate ceramic dielectric material being 100%, the added amount of Ho2O3 is 1.0-2.0 mol%, preferably 1.0-1.5 mol%.

4. The co-doped barium titanate ceramic dielectric material according to any one of claims 1 to 3, characterized in that: The average particle size of the co-doped barium titanate ceramic dielectric material is 160-230 nm.

5. A method for preparing the co-doped barium titanate ceramic dielectric material according to any one of claims 1 to 4, characterized in that: The preparation method comprises: The main material and MgO are mixed and wet ball-milled, dried, and then pre-calcined to obtain a pre-prepared powder; The prepared powder is mixed with the remaining doping materials except MgO and wet-milled, and then dried to obtain the co-doped barium titanate ceramic dielectric material.

6. The method for preparing the co-doped barium titanate ceramic dielectric material according to claim 5, characterized in that: The temperature of the pre-sintering treatment is 900-1100°C.

7. A multilayer ceramic capacitor, characterized in that: The multilayer ceramic capacitor is made of the co-doped barium titanate ceramic dielectric material according to any one of claims 1 to 4; The dielectric constant of the multilayer ceramic capacitor is 1400-1800 at 25°C.

8. The multilayer ceramic capacitor according to claim 7, wherein: The multilayer ceramic capacitor has a capacitance change rate between -15% and 15% at -55°C to 125°C.

9. A method for preparing a multilayer ceramic capacitor according to claim 7 or 8, characterized in that: The preparation method comprises: The multilayer ceramic capacitor is manufactured by sintering the co-doped barium titanate ceramic dielectric material in a reducing atmosphere.

10. The method for preparing a multilayer ceramic capacitor according to claim 9, characterized in that: The sintering temperature is 1150°C-1250°C.

Citation Information

Patent Citations

  • Chemical coating prepared base metal internal electrode multi-layer ceramic chip capacitor dielectric material

    CN101183610A

  • Base metal inner electrode multi-layer ceramic wafer type capacitor medium material prepared by chemical coating of water system

    CN101880167A

  • barium titanate-based X8R ceramic material and preparation method and ceramic capacitor thereof

    CN106966719A

  • High-voltage-withstanding barium-titanate-based composite ceramic dielectric material and preparation method thereof

    CN110117188A

  • Ceramic material as well as preparation method and application thereof

    CN113354410A

Cited By

  • Reduction-bias-resistant stable dielectric material and preparation method thereof

    CN120423873A