Photo-thermal-electric coupling adjustable high-entropy perovskite oxide functional ceramic as well as preparation method and application thereof

By introducing Er, Ni, and Nb ions into high-entropy perovskite oxide ceramics and using solid-phase preparation technology, the photothermal conversion temperature and sensitivity are improved, and the problem of insufficient temperature and sensitivity of existing materials is solved. It is suitable for multiple application fields.

CN118930255AActive Publication Date: 2024-11-12XIAN TECH UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411168521.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The temperature and sensitivity of existing photothermal conversion materials are relatively low, making it difficult to meet the demand for precise temperature control of photothermal therapy in biomedical science.

Method used

Develop a high-entropy perovskite oxide functional ceramic with adjustable light-thermal coupling. By introducing Er, Ni, and Nb ions, it uses 980nm laser excitation to increase the photothermal conversion temperature. and sensitivity, and reduce costs through solid phase preparation process, suitable for large-scale production.

Benefits of technology

It achieves higher photothermal conversion temperature and power sensitivity at lower power, and is suitable for contactless temperature sensing, display lighting, optical anti-counterfeiting and medicine, providing more efficient temperature control and detection capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930255A_ABST
    Figure CN118930255A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of multifunctional optical materials, and discloses a light-heat-electricity coupling adjustable high-entropy perovskite oxide functional ceramic and a preparation method and application thereof, the chemical formula of the functional ceramic is 0.6 (Bi0. 5Na0. 4K0. 1) 1-1.5 xErxTiO3-0. 4 [2 / 3 (SrTiO3)-1 / 3 (Bi (Mg2 / 3NiyNbz) O3)], x is more than or equal to 0 and less than or equal to 0.3, y is more than or equal to 0.1 and less than or equal to 0.5, z is more than or equal to 0.05 and less than or equal to 0.3, and 2y + 5z is more than or equal to 0.15 and less than or equal to 2.5. The entropy value is gt; and 1.61). The preparation method comprises the following steps: uniformly mixing Bi2O3, Na2CO3, TiO2, SrCO3, MgO, NiO, Nb2O5, Er2O3, K2CO3 and a solvent, pre-sintering, granulating, tabletting, and sintering. The functional ceramic has light-light, light-heat and light-electricity conversion functions and can be applied to the fields of non-contact temperature sensing, display illumination, optical anti-counterfeiting, optoelectronic devices and medicine, and the preparation method is low in cost and high in yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of multifunctional optical materials, and in particular relates to a high-entropy perovskite oxide functional ceramic with adjustable light-heat-electric coupling, a preparation method and an application thereof. Background Art

[0002] Upconversion luminescent materials can convert infrared light into visible light, and have a wide range of applications in important fields such as display and lighting, super-resolution imaging, temperature sensing, optical therapy, solid-state lasers, optical anti-counterfeiting, optoelectronic devices, etc., and have attracted widespread attention from scientists around the world. Upconversion luminescence has the advantages of high emission intensity, strong penetration, no lethality to biological tissues, and weak spontaneous background fluorescence, so it is widely used in the field of medical applications.

[0003] In recent years, the rapid development of temperature measurement relies on the non-invasive fluorescence intensity ratio (FIR) technology of the difference in photoluminescence (PL) emission peaks of luminescent materials at different temperatures. This technology has important advantages such as rapid detection and high sensitivity. Photothermal therapy (PTT) is a physical therapy that converts absorbed light energy into heat through photothermal therapeutic agents (PTAs). The performance of PTT is closely related to the heat production of PTAs, but insufficient heat at the treatment site or excessive body temperature may lead to ineffective treatment or unpredictable damage to surrounding normal tissues. By developing new materials with the dual functions of precise real-time intracellular temperature feedback and photothermal conversion, it is an effective way to control the temperature of the photothermal conversion process. The extensive research on new photothermal materials has become a frontier research field with a wide range of high-potential applications in physics, chemistry and life sciences. Rare earth ions (RE 3+ ) has abundant step-like energy levels as luminescence centers, which has become the focus of FIR research. This technology has been widely used as a non-invasive temperature detection technology to detect the temperature of PTA in biological systems. Functional ceramics have been integrated into human daily life due to their long-term safety and stability, such as applications in high temperature environments, scenes with high requirements for mechanical strength and wear resistance, environments with high requirements for chemical stability, and the manufacture of large-size parts. Moreover, its cost is low and it is suitable for industrial mass production. Therefore, it is necessary to study the photothermal properties of ceramics. Generally, photothermal ceramics with fluorescent properties are achieved by rare earth ion doping.

[0004] Traditional contact temperature detection is widely used in many fields, but its slow response speed and poor adaptability to complex environments (such as in vivo, strong magnetic fields and corrosive environments) are the main factors limiting its application. Therefore, non-contact temperature detection can not only avoid the above problems to a large extent, but also has the advantages of strong anti-interference and high signal resolution. The non-contact temperature sensor based on up-conversion luminescence adopts the characteristic that the specific energy level of rare earth ions has temperature-related radiation efficiency, and changes the intensity of up-conversion emission of rare earth ions through temperature changes, thereby realizing temperature detection. So far, the test technology based on fluorescence intensity ratio (FIR) rarely considers the error caused by the heat generated by the photothermal effect of the material itself on the detection result. This is because under most application conditions, the laser power is constant, so the error generated is controllable. However, in biomedicine, especially in photothermal therapy, it is necessary to change the power of the laser so that the material reaches the required photothermal temperature. Therefore, it is necessary to develop a power-driven non-contact temperature measurement system for materials with photothermal effect.

[0005] There are few reports on the application of fluorescent photothermal ceramics in power-driven FIR detection. In 2022, researchers introduced CCTO compounds to enhance the radiationless transition process of KNN-based ceramic materials containing Er ions, and studied its effect on the luminescence and photothermal properties of the material by adjusting the Yb doping content. The experiment obtained a photothermal conversion temperature of 70°C (at a driving power of 0.4W) and a power sensitivity of 0.61W. -1 , this system only adopts one photothermal conversion mechanism, and the resulting photothermal conversion temperature and sensitivity are relatively low. Summary of the invention

[0006] In order to solve the technical problems of relatively low photothermal conversion temperature and sensitivity in the prior art, the purpose of the present invention is to provide a high-entropy perovskite oxide functional ceramic with controllable photo-thermal-electric coupling and a preparation method and application, which has high photothermal conversion temperature and power sensitivity.

[0007] In order to achieve the above-mentioned invention object, the present invention provides the following technical solutions:

[0008] A high-entropy perovskite oxide functional ceramic with adjustable light-heat-electric coupling, wherein the chemical formula of the functional ceramic is 0.6(Bi 0.5 Na 0.4 K 0.1 ) 1-1.5x Er x TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni y Nb z)O3)], wherein 0≤x≤0.3, 0.1≤y≤0.5, 0.05≤z≤0.3, and 0.15≤2y+5z≤2.5; the entropy value range of the functional ceramic is: S>1.61.

[0009] A further improvement of the present invention is that 0.01≤x≤0.2, 0.2≤y≤0.4, 0.1≤z≤0.25, and 0.3≤2y+5z≤2.

[0010] A further improvement of the present invention is that 0.01≤x≤0.05, 0.3≤y≤0.4, 0.15≤z≤0.2, and 1.5≤2y+5z≤2.

[0011] A method for preparing a high-entropy perovskite oxide functional ceramic with controllable light-heat-electric coupling, comprising the following steps:

[0012] According to the chemical formula, 0.6(Bi 0.5 Na 0.4 k 0.1 ) 1-1.5x Er x TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3Ni y Nb z )O3)], Bi2O3, Na2CO3, TiO2, SrCO3, MgO, NiO, Nb2O5, Er2O3 and K2CO3 are uniformly mixed with a solvent, pre-sintered, granulated, pressed into tablets and then sintered to obtain a high-entropy perovskite oxide functional ceramic with controllable light-heat-electric coupling;

[0013] Among them, 0≤x≤0.3, 0.1≤y≤0.5, 0.05≤z≤0.3, and 0.15≤2y+5z≤2.5; and the entropy value range of the functional ceramics is: S>1.61.

[0014] A further improvement of the present invention is that 0.01≤x≤0.2, 0.2≤y≤0.4, 0.1≤z≤0.25, and 0.3≤2y+5z≤2.

[0015] A further improvement of the present invention is that 0.01≤x≤0.05, 0.3≤y≤0.4, 0.15≤z≤0.2, and 1.5≤2y+5z≤2.

[0016] The further improvement of the present invention lies in that the solvent is ethanol, isopropanol or acetone; the pre-burning temperature is 800°C-950°C and the time is 2 hours to 3 hours; and the binder is added before granulation.

[0017] A further improvement of the present invention is that the adhesive is a PVA solution with a mass fraction of 5%-10%; and after granulation, it is sieved through a 80-120 mesh screen.

[0018] A further improvement of the present invention is that the solvent is ethanol and the sintering process is: first sintering at 550°C-650°C for 2h-5h; and then sintering at 1100°C-1200°C for 1.5h-3h.

[0019] A high-entropy perovskite oxide functional ceramic with controllable light-heat-electric coupling is used in temperature sensing, display lighting, optical anti-counterfeiting, optoelectronic devices and medical fields.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention uses Bi2O3, Na2CO3, TiO2, SrCO3, MgO, NiO, Nb2O5, Er2O3 and K2CO3 as raw materials and utilizes a simple high temperature solid phase reaction method to prepare 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 1-1.5x Er x TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni y Nb z )O3)] ceramic material, compared with the existing process of preparing nano precursors by solution-gel method or hydrothermal method and then preparing ceramics, the functional ceramics of the present invention prepare precursors by solid phase method and then prepare ceramics. This method has low cost, high yield, simple process and is suitable for large-scale production.

[0022] The present invention adjusts the fluorescence intensity and light-to-heat conversion temperature characteristics of the material by focusing on adjusting the content of Er, Ni, and Nb ions. 3+ Ions and Ni 2+ When excited by 980nm laser, the ions will produce a dual effect of non-radiative transition and infrared self-absorption, which makes the material have a higher photothermal conversion temperature and based on Er 3+ Due to its unique energy level structure, functional ceramics can obtain specific up-conversion luminescence ability. At the same time, the NBT matrix material itself has good pyroelectric properties, which ultimately realizes the mutual coupling characteristics of the material system of functional ceramics to synergistically produce photothermal conversion, photoelectric conversion and up-conversion luminescence.

[0023] Since functional ceramics are fluorescent materials with photothermal properties, they can be used in the field of non-contact temperature sensing. By irradiating the ceramic material with 980nm infrared light, a higher photothermal conversion temperature and power sensitivity are obtained at a lower power. The ceramic material prepared by the present invention has the function of adjustable light-heat-electric coupling, and can be used in non-contact temperature sensing, display lighting, optical anti-counterfeiting, optoelectronic devices and medical fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The X-ray diffraction pattern of the ceramic sample provided in Example 1 of the present invention;

[0025] Figure 2 This is an excitation spectrum diagram of the ceramic sample provided in Example 1 of the present invention, wherein the wavelength of the emitted light is 980 nm;

[0026] Figure 3 This is a diagram of the central maximum temperature of the photothermal conversion of the ceramic sample provided in Example 1 of the present invention, with an excitation wavelength of 980nm and a power of 0.2W;

[0027] Figure 4 The X-ray diffraction pattern of the ceramic sample provided in Example 2 of the present invention;

[0028] Figure 5 This is an excitation spectrum diagram of the sample provided in Example 2 of the present invention, wherein the wavelength of the emitted light is 980nm;

[0029] Figure 6 This is a central maximum temperature diagram of the photothermal conversion of the sample provided in Example 3 of the present invention, with an excitation wavelength of 980nm and a power of 1W;

[0030] Figure 7 The X-ray diffraction pattern of the ceramic sample provided in Example 3 of the present invention;

[0031] Figure 8 This is a central maximum temperature diagram of the photothermal conversion of the sample provided in Example 3 of the present invention, with an excitation wavelength of 980nm and a power of 0.4W;

[0032] Fig. 9 This is a diagram of the central maximum temperature of the photothermal conversion of the sample provided in Example 3 of the present invention, with an excitation wavelength of 980nm and a power of 0.6W;

[0033] Fig.10 The X-ray diffraction pattern of the ceramic sample provided in Example 4 of the present invention;

[0034] Fig.11 This is an excitation spectrum diagram of the sample provided in Example 4 of the present invention, wherein the wavelength of the emitted light is 980nm;

[0035] Fig.12 This is a diagram of the central maximum temperature of the photothermal conversion of the ceramic sample provided in Example 4 of the present invention, with an excitation wavelength of 980nm and a power of 0.8W;

[0036] Fig.13 The dark current of the ceramic sample provided in Example 4 of the present invention at a voltage of up to 10V and the photocurrent under 980nm excitation.

[0037] Fig.14 The X-ray diffraction pattern of the ceramic sample provided in Comparative Example 1 of the present invention;

[0038] Fig.15 This is an excitation spectrum diagram of the sample provided in Comparative Example 1 of the present invention, wherein the wavelength of the emitted light is 980 nm;

[0039] Fig.16 This is a central maximum temperature diagram of the photothermal conversion of the ceramic sample provided in Comparative Example 1 of the present invention, with an excitation wavelength of 980nm and a power of 0.4W;

[0040] Fig.17 The X-ray diffraction pattern of the ceramic sample provided in Comparative Example 2 of the present invention;

[0041] Fig.18 This is the central maximum temperature diagram of the photothermal conversion of the ceramic sample provided in Comparative Example 2 of the present invention, with an excitation wavelength of 980nm and a power of 0.4W. DETAILED DESCRIPTION

[0042] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly and comprehensively understood.

[0043] Sodium bismuth titanate (Bi 0.5 Na 0.5 TiO3, BNT) material is a multifunctional A-site composite ion perovskite ferroelectric. Compared with other materials, it has lower requirements for the atmosphere and temperature of the sintering environment, good chemical stability, no strict requirements for humidity, can be stored for a long time, and has good repeatability in the preparation process, so it can be applied to large-scale industrial production. The Curie temperature is relatively high (320°C) and the relative dielectric constant is relatively small (240-340°C), so it can be applied to high temperature conditions. Based on the high entropy theory, the present invention utilizes the introduction of multiple elements to prepare high entropy perovskite oxide functional ceramics, and realizes the adjustability of light-heat-electric coupling through the synergistic effect of multiple mechanisms.

[0044] Since the phonon energy of BNT-based ceramics is low and there are defect states such as vacancies inside, it can effectively increase the radiation transitions within the material system and the cross-relaxation effects between related energy levels, thereby increasing the number of particles at the effective luminescent energy level, thereby enhancing the system's upconversion luminescence ability and photothermal conversion ability.

[0045] The chemical formula of the light-heat-electric coupling-adjustable high-entropy perovskite oxide functional ceramic with light-heat-electric coupling characteristics of the present invention is 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 1-1.5x Er x TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3Ni y Nb z )O3)], wherein x, y, z represent the molar fractions of the corresponding elements, and 0≤x≤0.3, 0.1≤y≤0.5, 0.05≤z≤0.3, and 0.15≤2y+5z≤2.5; at the same time, the entropy value S of the functional ceramics ranges from S>1.61.

[0046] Preferably, the value range of x, y, z is 0.01≤x≤0.2, 0.2≤y≤0.4, 0.1≤z≤0.25, and 0.3≤2y+5z≤2; meanwhile, the oxide entropy value range is: S>1.61. Reason for preference: Within this range, the obtained functional ceramics have better performance.

[0047] Further preferably, 0.01≤x≤0.05, 0.3≤y≤0.4, 0.15≤z≤0.2, 1.5≤2y+5z≤2; meanwhile, the entropy value range of the functional ceramic is: S>1.61.

[0048] The method for preparing the light-heat-electric coupling controllable high-entropy perovskite oxide functional ceramics with light-heat-electric coupling characteristics of the present invention comprises the following steps:

[0049] Bi2O3, Na2CO3, TiO2, SrCO3, MgO, NiO, Nb2O5, Er2O3 and K2CO3 are used as raw materials, the above raw materials are mixed in proportion, ethanol is used as a solvent, and the mixed powder is ground in a ball mill, and then the powder is dried and pre-fired; then the pre-fired powder is ground again, a binder is added and granulated, and after tableting, low-temperature plastic removal and high-temperature sintering are performed, and the powder is cooled to room temperature to obtain a light-heat-electric coupling-adjustable high-entropy perovskite oxide functional ceramic with light-heat-electric coupling characteristics, that is, 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 1-1.5x Erx TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni y Nb z )O3)]ceramics.

[0050] When mixed, the mass ratio of raw material: ethanol: zirconium ball = 1:1:2.

[0051] The ball mill is a planetary ball mill, and the ball milling time is more than 6 hours.

[0052] The pre-calcination is performed at 800°C-950°C for 2 hours to 3 hours;

[0053] The adhesive is a PVA solution with a mass fraction of 5%.

[0054] During the granulation process, the powder is passed through a 80-120 mesh sieve.

[0055] In the tableting process, a SDY-20 manual and electric tablet press is used to press the powder into shape at a pressure of 5-20 MPa.

[0056] The sintering is first performed at low temperature and then at high temperature. The temperature of the low temperature is 550°C-650°C and the time is 2h-5h; the temperature of the high temperature is 1100°C-1200°C and the time is 1.5h-3h.

[0057] In the present invention, unless otherwise specified, the raw materials used are all commercially available products in the art. The present invention has no particular limitation on the amount of the raw materials, as long as the general chemical formula is satisfied.

[0058] Compared with the existing process of preparing nano precursors by solution-gel method or hydrothermal method and then preparing ceramics, the functional ceramics of the present invention prepare precursors by solid phase method and then prepare ceramics. This method has low cost, high yield, simple process and is suitable for large-scale production.

[0059] The raw materials used are all commercially available, the raw materials are easy to obtain, the process is simple, the quality of the obtained products is stable and reliable, and it is conducive to industrial production.

[0060] The high entropy perovskite oxide functional ceramic has a broad emission peak at 500nm-700nm when the sample is irradiated with a laser of 960nm-990nm.

[0061] Furthermore, under 980nm laser irradiation with a power of more than 1mW, the sample (i.e., high entropy perovskite oxide functional ceramic) has broad emission peaks at green light near 520nm and 550nm and red light near 650nm, and generates heat. As the laser power increases, the photothermal conversion temperature begins to rise continuously, and the fluorescence intensity ratio (FIR) of the two emission peaks at 520nm and 550nm changes. Fitting and analyzing the FIR data can obtain the material-related power sensitivity.

[0062] When the ceramic is irradiated with a laser of 800nm-990nm, the light-heat conversion phenomenon is generated by adjusting the laser power, and the fluorescence intensity ratio obtained by the ceramic at different powers changes.

[0063] The light-heat-electric coupling regulatable high-entropy perovskite oxide functional ceramics prepared by the above preparation method of the present invention are fluorescent materials with light-light, light-heat, and light-electric conversion functions, and can be used in temperature sensing, display lighting, optical anti-counterfeiting, optoelectronic devices and medical fields. Furthermore, the ceramics can be used in the field of non-contact temperature sensing.

[0064] In order to further illustrate the present invention, the light-heat-electric coupling controllable high-entropy perovskite oxide functional ceramics provided by the present invention and their preparation methods and applications are described in detail below in combination with examples, but they should not be understood as limiting the scope of protection of the present invention.

[0065] The present invention will now be further described in conjunction with specific embodiments.

[0066] Example 1

[0067] x is 0.01, y is 1 / 3, z is 0, that is, 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 0.985 Er 0.01 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni 1 / 3 )O3)], the entropy value is 1.70.

[0068] The preparation method of the functional ceramic 1 is as follows:

[0069] Commercially available high-purity Bi2O3, Na2CO3, TiO2, SrCO3, NiO, MgO, Er2O3 and K2CO3 are used as raw materials, and the mass of each oxide is accurately weighed according to the above formula. The weighed raw materials are placed in a clean agate jar, and anhydrous ethanol is used as a solvent. The mass ratio of raw materials: ethanol: zirconium balls = 1:1:2 is ground on a planetary ball mill to make a uniformly mixed powder for 12 hours. The above powder is then dried in an oven, placed in a corundum crucible, placed in a box furnace, and continuously heated to 900℃ for pre-sintering for 2 hours, and then cooled to 600℃. After that, the product obtained after cooling in the furnace is ground with an agate mortar, and a PVA solution with a mass fraction of 5% of the binder is added. It is fully ground, mixed evenly, granulated, and passed through an 80-120 mesh sieve. The powder is pressed into a ceramic green sheet with a diameter of 10mm using a SDY-20 manual and electric tablet press at a pressure of 5MPa. The ceramic green sheet was placed in a high temperature furnace, heated continuously, kept at 600°C for 180 minutes to discharge the plastic, then heated continuously, sintered at 1190°C for 2 hours, cooled to 600°C, and naturally cooled to obtain 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 0.985 Er 0.01 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni 1 / 3 )O3)]ceramic materials.

[0070] See also Figure 1 , it can be seen that the ceramic sample is a single perovskite structure;

[0071] See also Figure 2 , it can be seen that the ceramic sample has generation peaks at 520nm 550nm 660nm under 980nm laser excitation;

[0072] See also Figure 3 It can be seen that the maximum temperature at the center of the ceramic surface changes with time when irradiated with a 980nm laser at a power of 0.2W. The temperature rises to 60.5℃ and then enters a stable stage.

[0073] Example 2

[0074] x is 0.02, y is 0, z is 1 / 3, that is, 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 0.97 Er 0.02 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni 1 / 3 )O3)], the entropy value is 1.70.

[0075] The preparation method of functional ceramic 2 is as follows:

[0076] Commercially available high-purity Bi2O3, Na2CO3, TiO2, SrCO3, NiO, MgO, Er2O3 and K2CO3 are used as raw materials, and the mass of each oxide is accurately weighed according to the above formula. The weighed raw materials are placed in a clean agate jar, and anhydrous ethanol is used as a solvent. The mass ratio of raw materials: ethanol: zirconium balls = 1:1:2 is ground on a planetary ball mill to make a uniformly mixed powder for 18 hours. Then the above powder is dried in an oven, then placed in a corundum crucible, placed in a box furnace, and continuously heated to 900℃ for pre-burning for 2 hours, and then cooled to 600℃. After that, the product obtained after cooling in the furnace is ground with an agate mortar, and a PVA solution with a mass fraction of 5% of the binder is added. It is fully ground, mixed evenly, granulated, and passed through an 80-120 mesh sieve. The powder is pressed into a ceramic green sheet with a diameter of 10mm using a SDY-20 manual and electric tablet press at a pressure of 20MPa. The ceramic green sheet was placed in a high temperature furnace, heated continuously, kept at 600°C for 180 minutes to discharge the plastic, then heated continuously, sintered at 1180°C for 2 hours, cooled to 600°C, and naturally cooled to obtain 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 0.97 Er 0.02 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3Ni 1 / 3 )O3)]ceramic materials.

[0077] See also Figure 4 , it can be seen that the ceramic sample has a perovskite main phase.

[0078] See also Figure 5 , it can be seen that the ceramic sample has emission peaks at 520nm 550nm 660nm under 980nm laser excitation, and the peak at red light is wider;

[0079] See also Figure 6 It can be seen that the maximum temperature at the center of the ceramic surface changes with time when irradiated with a 980nm laser at a power of 1W. The temperature rises to 227℃ and then enters a stable stage.

[0080] Example 3

[0081] x is 0.03, y is 1 / 3, z is 0.1, that is, 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 0.955 Er 0.03TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni 1 / 3 Nb 0.1 )O3)], the entropy value is 1.75.

[0082] The preparation method of functional ceramic 3 is as follows:

[0083] Commercially available high-purity Bi2O3, Na2CO3, TiO2, SrCO3, NiO, MgO, Nb2O5, Er2O3 and K2CO3 are used as raw materials, and the mass of each oxide is accurately weighed according to the above formula. The weighed raw materials are placed in a clean agate jar, and anhydrous ethanol is used as a solvent. The mass ratio of raw materials: ethanol: zirconium balls = 1:1:2 is ground on a planetary ball mill to make a uniformly mixed powder for 24 hours. The above powder is then dried in an oven, placed in a corundum crucible, placed in a box furnace, and continuously heated to 850℃ for pre-burning for 2 hours, and then cooled to 600℃. After that, the product obtained after cooling in the furnace is ground with an agate mortar, and a PVA solution with a mass fraction of 5% of the binder is added. It is fully ground, mixed evenly, granulated, and passed through an 80-120 mesh sieve. The powder is pressed into a ceramic green sheet with a diameter of 10mm using a SDY-20 manual and electric tablet press at a pressure of 20MPa. The ceramic green sheet was placed in a high temperature furnace, heated continuously, kept at 600°C for 180 minutes to remove the plastic, then heated continuously, sintered at 1170°C for 2.5 hours, cooled to 600°C, and naturally cooled to obtain .6(Bi 0.5 Na 0.4 K 0.1 ) 0.955 Er 0.03 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni 1 / 3 Nb 0.1 )O3)]ceramic materials.

[0084] See also Figure 7 , it can be seen that the ceramic sample is a single perovskite structure.

[0085] See also Figure 8 It can be seen that the maximum temperature at the center of the ceramic surface changes with time when the 980nm laser is irradiated at a power of 0.4W. The temperature rises to 98℃ and then enters a stable stage.

[0086] See also Fig. 9 It can be seen that the maximum temperature at the center of the ceramic surface changes with time when the 980nm laser is irradiated at a power of 0.6W. The temperature rises to 131℃ and then enters a stable stage.

[0087] Example 4

[0088] x is 0.1, y is 1 / 3, z is 0, that is, 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 0.85 Er 0.1 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni 1 / 3 )O3)], the entropy value is 1.75.

[0089] The preparation method of functional ceramic 4 is as follows:

[0090] Commercially available high-purity Bi2O3, Na2CO3, TiO2, SrCO3, NiO, MgO, Er2O3 and K2CO3 are used as raw materials, and the mass of each oxide is accurately weighed according to the above formula. The weighed raw materials are placed in a clean agate jar, and anhydrous ethanol is used as a solvent. The mass ratio of raw materials: ethanol: zirconium balls = 1:1:2 is ground on a planetary ball mill to make a uniformly mixed powder for 12 hours. The above powder is then dried in an oven, placed in a corundum crucible, placed in a box furnace, and continuously heated to 900℃ for pre-sintering for 2 hours, and then cooled to 600℃. After that, the product obtained after cooling in the furnace is ground with an agate mortar, and a PVA solution with a mass fraction of 5% of the binder is added. It is fully ground, mixed evenly, granulated, and passed through an 80-120 mesh sieve. The powder is pressed into a ceramic green sheet with a diameter of 10mm using a SDY-20 manual and electric tablet press at a pressure of 20MPa. The ceramic green sheet was placed in a high temperature furnace, heated continuously, kept at 600°C for 180 minutes to discharge the plastic, then heated continuously, sintered at 1190°C for 2 hours, cooled to 600°C, and naturally cooled to obtain 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 0.85 Er 0.1 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3Ni 1 / 3 )O3)]ceramic materials.

[0091] See also Fig.10 , it can be seen that the ceramic sample has a perovskite main phase.

[0092] See also Fig.11 , it can be seen that the ceramic sample has emission peaks at 520nm 550nm 660nm under 980nm laser excitation;

[0093] See also Fig.12It can be seen that when using a 980nm laser and irradiating at a power of 0.8W, the maximum temperature at the center of the ceramic surface changes with time. After the temperature rises to 150℃, it enters a stable stage.

[0094] See also Fig.13 , it can be seen that the dark current of the ceramic sample at a maximum voltage of 10V and the photocurrent under 980nm excitation.

[0095] Example 5

[0096] x is 0.02, y is 1 / 3, z is 1 / 5, that is, 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 0.985 Er 0.01 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni 1 / 3 Nb 1 / 5 )O3)], the entropy value is 1.80.

[0097] The preparation method of functional ceramic 5 is as follows:

[0098] Commercially available high-purity Bi2O3, Na2CO3, TiO2, SrCO3, NiO, MgO, Nb2O5, Er2O3 and K2CO3 are used as raw materials, and the mass of each oxide is accurately weighed according to the above formula. The weighed raw materials are placed in a clean agate jar, and anhydrous ethanol is used as a solvent. The mass ratio of raw materials: ethanol: zirconium balls = 1:1:2 is ground on a planetary ball mill to make a uniformly mixed powder for 12 hours. Then the above powder is dried in an oven, then placed in a corundum crucible, placed in a box furnace, and continuously heated to 850℃ for pre-calcination for 2.5 hours, and then cooled to 600℃. After that, the product obtained after cooling in the furnace is ground with an agate mortar, and a PVA solution with a mass fraction of 5% of the binder is added. It is fully ground, mixed evenly, granulated, and passed through an 80-120 mesh sieve. The powder is pressed into a ceramic green sheet with a diameter of 10mm using a SDY-20 manual and electric tablet press at a pressure of 20MPa. The ceramic green sheet was placed in a high temperature furnace, heated continuously, kept at 600°C for 180 minutes to discharge the plastic, then heated continuously, sintered at 1180°C for 2 hours, cooled to 600°C, and naturally cooled to obtain 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 0.985 Er 0.01 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni 1 / 3 Nb 1 / 5 )O3)]ceramic materials.

[0099] Example 6

[0100] x is 0.2, y is 1 / 2, z is 4 / 15, that is, 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 0.7 Er 0.2 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni 1 / 2 Nb 4 / 15 )O3)], the entropy value is 1.79.

[0101] The preparation method of functional ceramic 6 is as follows:

[0102] Commercially available high-purity Bi2O3, Na2CO3, TiO2, SrCO3, NiO, MgO, Nb2O5, Er2O3 and K2CO3 are used as raw materials, and the mass of each oxide is accurately weighed according to the above formula. The weighed raw materials are placed in a clean agate jar, and anhydrous ethanol is used as a solvent. The mass ratio of raw materials: ethanol: zirconium balls = 1:1:2 is ground on a planetary ball mill to make a uniformly mixed powder for 18 hours. Then the above powder is dried in an oven, then placed in a corundum crucible, placed in a box furnace, and continuously heated to 900℃ for pre-burning for 2 hours, and then cooled to 600℃. After that, the product obtained after cooling in the furnace is ground with an agate mortar, and a PVA solution with a mass fraction of 5% of the binder is added. It is fully ground, mixed evenly, granulated, and passed through an 80-120 mesh sieve. The powder is pressed into a ceramic green sheet with a diameter of 10mm using a SDY-20 manual and electric tablet press at a pressure of 20MPa. The ceramic green sheet was placed in a high temperature furnace, heated continuously, kept at 600°C for 180 minutes to discharge the plastic, then heated continuously, sintered at 1180°C for 2 hours, cooled to 600°C, and naturally cooled to obtain 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 0.7 Er 0.2 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3Ni 1 / 2 Nb 4 / 15 )O3)]ceramic materials.

[0103] Example 7

[0104] x is 0, y is 0.1, z is 0.05, that is, 0.6 (Bi 0.5 Na 0.4 K 0.1 )TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3Ni0.1 Nb 0.05 )O3)], the entropy value is 1.65.

[0105] The preparation method of the functional ceramic 7 is as follows:

[0106] Commercially available high-purity Bi2O3, Na2CO3, TiO2, SrCO3, NiO, MgO, Er2O3 and K2CO3 are used as raw materials, and the mass of each oxide is accurately weighed according to the above formula. The weighed raw materials are placed in a clean agate jar, and anhydrous ethanol is used as a solvent. The mass ratio of raw materials: ethanol: zirconium balls = 1:1:2 is ground on a planetary ball mill to make a mixed powder for 6 hours. Then the above powder is dried in an oven, then placed in a corundum crucible, put into a box furnace, and continuously heated to 870℃ for pre-calcination for 2.5 hours, and then cooled to 600℃. After that, the product obtained after cooling in the furnace is ground with an agate mortar, and a PVA solution with a mass fraction of 5% of the binder is added. It is fully ground, mixed evenly, granulated, and passed through an 80-120 mesh sieve. The powder is pressed into a ceramic green sheet with a diameter of 10mm using a SDY-20 manual and electric tablet press at a pressure of 5MPa. The ceramic green sheet is placed in a high-temperature furnace, the temperature is continuously increased, and the temperature is kept at 550°C for 5 hours to discharge the plastic. Then the temperature is continuously increased, and sintered at 1100°C for 3 hours. The temperature is reduced to 600°C, and after natural cooling, a high-entropy perovskite oxide functional ceramic with controllable light-heat-electric coupling is obtained.

[0107] Example 8

[0108] x is 0.3, y is 0.2, z is 0.15, that is, 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 0.55 Er 0.3 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni 0.2 Nb 0.15 )O3)], the entropy value is 1.61.

[0109] The preparation method of functional ceramic 8 is as follows:

[0110] Commercially available high-purity Bi2O3, Na2CO3, TiO2, SrCO3, NiO, MgO, Er2O3 and K2CO3 are used as raw materials, and the mass of each oxide is accurately weighed according to the above formula. The weighed raw materials are placed in a clean agate jar, and anhydrous ethanol is used as a solvent. The mass ratio of raw materials: ethanol: zirconium balls = 1:1:2 is ground on a planetary ball mill to make a mixed powder for 10 hours. Then the above powder is dried in an oven, then placed in a corundum crucible, put into a box furnace, and continuously heated to 900℃ for pre-burning for 2 hours, and then cooled to 600℃. After that, the product obtained after cooling in the furnace is ground with an agate mortar, and a PVA solution with a mass fraction of 5% of the binder is added. It is fully ground, mixed evenly, granulated, and passed through an 80-120 mesh sieve. The powder is pressed into a ceramic green sheet with a diameter of 10mm using a SDY-20 manual and electric tablet press at a pressure of 5MPa. The ceramic green sheet is placed in a high-temperature furnace, the temperature is continuously increased, and the temperature is kept at 650°C for 2 hours to discharge the plastic. Then the temperature is continuously increased, sintered at 1200°C for 1.5 hours, cooled to 600°C, and naturally cooled to obtain high-entropy perovskite oxide functional ceramics with controllable light-heat-electric coupling.

[0111] Example 9

[0112] x is 0.05, y is 0.4, z is 0.25, that is, 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 0.925 Er 0.05 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni 0.4 Nb 0.25 )O3)], the entropy value is 1.82.

[0113] The preparation method of the functional ceramic 9 is as follows:

[0114] Commercially available high-purity Bi2O3, Na2CO3, TiO2, SrCO3, NiO, MgO, Er2O3 and K2CO3 are used as raw materials, and the mass of each oxide is accurately weighed according to the above formula. The weighed raw materials are placed in a clean agate jar, and anhydrous ethanol is used as a solvent. The mass ratio of raw materials: ethanol: zirconium balls = 1:1:2 is ground on a planetary ball mill to make a mixed powder for 20 hours. Then the above powder is dried in an oven, then placed in a corundum crucible, placed in a box furnace, and continuously heated to 820℃ for pre-burning for 3 hours, and then cooled to 600℃. After that, the product obtained after cooling in the furnace is ground with an agate mortar, and a PVA solution with a mass fraction of 5% of the binder is added. It is fully ground, mixed evenly, granulated, and passed through an 80-120 mesh sieve. The powder is pressed into a ceramic green sheet with a diameter of 10mm using a SDY-20 manual and electric tablet press at a pressure of 5MPa. The ceramic green sheet is placed in a high-temperature furnace, the temperature is continuously increased, and the temperature is kept at 620°C for 3 hours to discharge the plastic. Then the temperature is continuously increased, sintered at 1140°C for 2 hours, cooled to 600°C, and naturally cooled to obtain high-entropy perovskite oxide functional ceramics with controllable light-heat-electric coupling.

[0115] Comparative Example 1

[0116] x is 0.01, y is 0, z is 1 / 3, that is, 0.6 (Bi 0.5 Na 0.4 K 0.1 ) 0.985 Er 0.01 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Nb 1 / 3 )O3)], the entropy value is 1.70.

[0117] The preparation method of the functional ceramic 10 is as follows:

[0118] Commercially available high-purity Bi2O3, Na2CO3, TiO2, SrCO3, Nb2O 5、MgO, Er2O3 and K2CO3 are used as raw materials, and the mass of each oxide is accurately weighed according to the above formula. The weighed raw materials are placed in a clean agate jar, and anhydrous ethanol is used as the solvent. The mass ratio of raw materials: ethanol: zirconium balls = 1:1:2 is used for grinding on a planetary ball mill to make a uniformly mixed powder for 20 hours. Then the above powder is dried in an oven, then placed in a corundum crucible, put into a box furnace, and continuously heated to 820℃ for pre-burning for 3 hours, and then cooled to 600℃. After that, the product obtained after cooling with the furnace is ground with an agate mortar, and a PVA solution with a mass fraction of 5% of the binder is added. It is fully ground, mixed evenly, granulated, and passed through an 80-120 mesh sieve. The powder is pressed into a ceramic green sheet with a diameter of 10mm using a SDY-20 manual and electric tablet press at a pressure of 5MPa. The ceramic green sheet is placed in a high-temperature furnace, the temperature is continuously increased, and the temperature is kept at 620°C for 3 hours to discharge the plastic. Then the temperature is continuously increased, sintered at 1140°C for 2 hours, cooled to 600°C, and naturally cooled to obtain high-entropy perovskite oxide functional ceramics with controllable light-heat-electric coupling.

[0119] See also Fig.14 , it can be seen that the ceramic sample has a perovskite main phase.

[0120] See also Fig.15 , it can be seen that the ceramic sample has emission peaks at 520nm 550nm 660nm under 980nm laser excitation;

[0121] See also Fig.16 It can be seen that when using 980nm laser and irradiating at 0.4W power, the maximum temperature at the center of the ceramic surface changes with time. After the temperature rises to 40℃, it enters a stable stage.

[0122] The addition of rare earth ion Er makes the material system have up-conversion luminescence characteristics under the action of 980nm laser, but the photothermal effect is not strong. The test results show that the relative photothermal conversion is only about 10℃.

[0123] Comparative Example 2

[0124] x is 0, y is 0, z is 1 / 3, that is, 0.6Bi 0.5 Na 0.4 K 0.1 TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Nb 1 / 3 )O3)], the entropy value is 1.70.

[0125] The preparation method of the functional ceramic 11 is as follows:

[0126] Commercially available high-purity Bi2O3, Na2CO3, TiO2, SrCO3, Nb2O5, MgO and K2CO3 are used as raw materials, and the mass of each oxide is accurately weighed according to the above formula. The weighed raw materials are placed in a clean agate jar, and anhydrous ethanol is used as a solvent. The mass ratio of raw materials: ethanol: zirconium balls = 1:1:2 is used for grinding on a planetary ball mill to make a uniformly mixed powder for 20 hours. Then the above powder is dried in an oven, then placed in a corundum crucible, placed in a box furnace, and continuously heated to 820℃ for pre-burning for 3 hours, and then cooled to 600℃. After that, the product obtained after cooling in the furnace is ground with an agate mortar, and a PVA solution with a mass fraction of 5% of the binder is added. It is fully ground, mixed evenly, granulated, and passed through an 80-120 mesh sieve. The powder is pressed into a ceramic green sheet with a diameter of 10mm using a SDY-20 manual and electric tablet press at a pressure of 5MPa. The ceramic green sheet is placed in a high-temperature furnace, the temperature is continuously increased, and the temperature is kept at 620°C for 3 hours to discharge the plastic. Then the temperature is continuously increased, sintered at 1140°C for 2 hours, cooled to 600°C, and naturally cooled to obtain high-entropy perovskite oxide functional ceramics with controllable light-heat-electric coupling.

[0127] See also Fig.17 , it can be seen that the ceramic sample has a perovskite main phase.

[0128] See also Fig.18 It can be seen that when using 980nm laser and irradiating at 0.4W power, the maximum temperature at the center of the ceramic surface changes with time, and the temperature rise is very small.

[0129] When the rare earth element Er is not added to the material system, there is no up-conversion luminescence characteristic, only a weak photothermal effect exists, and the sample temperature rises by about 10°C; when both Er and Ni elements are absent, affected by the laser's own radiation field and the environmental field, the test results only show a small temperature disturbance, and there is almost no photothermal effect in the material system.

[0130] In the present invention, the light-heat conversion temperature and luminous intensity of the system are regulated by regulating the contents of Er, Nb, and Nb, and utilizing the internal energy transfer mechanism and infrared self-absorption characteristics of the ceramic. The light-heat-electric coupling characteristics of the material system are regulated by regulating the defect concentration of the system and the comprehensive effect of the high-entropy oxide constituent elements on the perovskite ceramic crystal field.

[0131] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. However, all changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.

[0132] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.

Claims

1. A high-entropy perovskite oxide functional ceramic with controllable light-heat-electric coupling, characterized in that: The chemical formula of the functional ceramic is 0.6(Bi 0.5 Na 0.4 K 0.1 ) 1-1.5x Er x TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni y Nb z )O3)], wherein 0≤x≤0.3, 0.1≤y≤0.5, 0.05≤z≤0.3, and 0.15≤2y+5z≤2.5; the entropy value range of the functional ceramic is: S>1.

61.

2. The light-heat-electric coupling controllable high-entropy perovskite oxide functional ceramic according to claim 1, characterized in that: 0.01≤x≤0.2, 0.2≤y≤0.4, 0.1≤z≤0.25, and 0.3≤2y+5z≤2.

3. The light-heat-electric coupling controllable high-entropy perovskite oxide functional ceramic according to claim 1, characterized in that: 0.01≤x≤0.05, 0.3≤y≤0.4, 0.15≤z≤0.2, and 1.5≤2y+5z≤2.

4. A method for preparing a high-entropy perovskite oxide functional ceramic with controllable light-heat-electric coupling, characterized in that: The following steps are involved: According to the chemical formula, 0.6(Bi 0.5 Na 0.4 k 0.1 ) 1-1.5x Er x TiO3-0.4[2 / 3(SrTiO3)-1 / 3(Bi(Mg 2 / 3 Ni y Nb z )O3)], Bi2O3, Na2CO3, TiO2, SrCO3, MgO, NiO, Nb2O5, Er2O3 and K2CO3 are uniformly mixed with a solvent, pre-sintered, granulated, pressed into tablets and then sintered to obtain a high-entropy perovskite oxide functional ceramic with controllable light-heat-electric coupling; Among them, 0≤x≤0.3, 0.1≤y≤0.5, 0.05≤z≤0.3, and 0.15≤2y+5z≤2.5; and the entropy value range of the functional ceramics is: S>1.

61.

5. The method for preparing the light-heat-electric coupling controllable high-entropy perovskite oxide functional ceramic according to claim 4, characterized in that: 0.01≤x≤0.2, 0.2≤y≤0.4, 0.1≤z≤0.25, and 0.3≤2y+5z≤2.

6. The method for preparing the light-heat-electric coupling controllable high-entropy perovskite oxide functional ceramic according to claim 4, characterized in that: 0.01≤x≤0.05, 0.3≤y≤0.4, 0.15≤z≤0.2, and 1.5≤2y+5z≤2.

7. The method for preparing the light-heat-electric coupling controllable high-entropy perovskite oxide functional ceramic according to claim 4, characterized in that: The solvent is ethanol, isopropanol or acetone; the pre-burning temperature is 800°C-950°C, and the time is 2 hours to 3 hours; and the binder is added before granulation.

8. The method for preparing the light-heat-electric coupling controllable high-entropy perovskite oxide functional ceramic according to claim 7, characterized in that: The adhesive is a PVA solution with a mass fraction of 5%-10%; after granulation, the solution is sieved through a 80-120 mesh screen.

9. The method for preparing the light-heat-electric coupling controllable high-entropy perovskite oxide functional ceramic according to claim 4, characterized in that: The solvent is ethanol, and the sintering process is: first sinter at 550°C-650°C for 2h-5h; and then sinter at 1100°C-1200°C for 1.5h-3h.

10. Application of a high-entropy perovskite oxide functional ceramic with controllable light-heat-electric coupling prepared by the method of any one of claims 1 to 3 or any one of claims 4 to 9 in the fields of temperature sensing, display lighting, optical anti-counterfeiting, optoelectronic devices and medicine.

Citation Information

Patent Citations

  • BNT-base lead-free electrostriction material with light-emitting characteristic and preparation method thereof

    CN104944943A

  • Electrically tunable up-conversion luminescence lead-free ferroelectric monocrystal material and preparation method thereof

    CN106012016A

  • Photochromic optical storage material and preparation method thereof

    CN108840674A

  • Compact NBT-KBT-BT-based multifunctional ceramic material with strong fluorescence and high piezoelectric properties and preparation method thereof

    CN111018518A

  • Sodium bismuth titanate-based dielectric ceramic with energy storage and fluorescence characteristics and preparation method thereof

    CN117623765A