Inorganic composite material as well as preparation method and application thereof

By adjusting the size of α-SiC particles and the fiber addition amount, an inorganic composite material with high compressive strength and elastic modulus was prepared, which solved the problem of the prone to deformation of the deep-sea pressure-resistant container material under high pressure, and improved the safety of the material and Finished rate.

CN118930295AInactive Publication Date: 2024-11-12SHANGHAI JINGWU SEA MATERIAL TECHNOLOGY DEVELOPMENT CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310527446.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing deep-sea pressure-resistant container materials are susceptible to compression deformation under high pressure, resulting in water leakage accidents. Traditional composite materials lack safety when working underwater, making it difficult to meet the needs of high elastic modulus and compressive strength.

Method used

Using an inorganic composite material composed of α-SiC, α-SiC fibers, β-SiC and silicon phases, the microstructure of the material is uniform at the millimeter level and uneven at the micrometer level by adjusting the size of the α-SiC particles and the amount of fibers added. Improve the compressive strength, elastic modulus and safety of the material.

Benefits of technology

A material with a density of 3.00-3.12g/cm3, a compressive strength of 3600-4000Mpa, and an elastic modulus of 390-410GPa has been realized. The deep-sea pressure-resistant container has safety and high performance when working underwater, and the finished product of large-size products is High rate and shrinkage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930295A_ABST
    Figure CN118930295A_ABST
Patent Text Reader

Abstract

The invention discloses an inorganic composite material as well as a preparation method and application thereof. The invention provides a preparation method of an inorganic composite material. The preparation method comprises the following steps: uniformly mixing alpha-SiC particles, alpha-SiC fibers and phenolic resin, performing spray drying to obtain spherical particles, pressing the spherical particles into a biscuit, and distributing silicon particles on and under the biscuit for siliconizing treatment. Under the action of high temperature, melt silicon permeates into a biscuit through gaps, holes are filled to form a continuous silicon phase, a sintered compact is formed, organic matter such as phenolic resin is carbonized into carbon powder, and secondary SiC (beta-SiC) is generated after the carbon powder reacts with silicon to be connected with original SiC. Therefore, the structure is composed of four phases, namely the alpha-SiC, the alpha-SiC fibers, the beta-SiC and the silicon phase, the beta-SiC and the silicon phase are a newly generated connecting phase and a gap filling phase, the density and the mechanical property of the composite material are improved through the microstructure, and the macroscopic uniformity of the material is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an inorganic composite material, a preparation method and application thereof. Background Art

[0002] At present, deep-sea pressure vessels, especially instrument cabins and other application fields, mostly use aluminum alloys, titanium alloys and stainless steel and other metal materials. In the deep sea more than 6,000 meters, large-sized (cylinders with an outer diameter of more than 300mm) metal containers cannot meet the application requirements because their elastic modulus is not high enough (aluminum alloy is 70GPa) and the compressive strength is low, which makes them easy to deform under pressure and often leaks. Therefore, materials with high elastic modulus (greater than 300GPa) are increasingly attracting the attention of experts in the marine field; deep-sea pressure vessels also urgently need materials with high elastic modulus and high compressive strength.

[0003] Composite materials have been developed in recent decades. Their advantages are excellent comprehensive performance and the ability to adjust certain specific properties according to different usage environments. In the process of pursuing the maximization of tensile strength, flexural strength and compressive strength of composite materials for many years, materials scientists have been involved in the study of composite material organization structure. Most of them pursue fine and uniform composite material microstructures from micron level to nanometer level and then to angstrom level (such as single crystal). The highest goal of this pursuit is that composite materials should not only exert their intrinsic highest performance but also be isotropic. At present, most materials workers are conducting research around this goal.

[0004] Deep-sea pressure-resistant materials and materials for mechanical seals, bulletproof, and kiln tools are two completely different application fields, so the requirements for composite materials are also different; traditional deep-sea pressure-resistant containers made of composite materials that pursue isotropy and fine and uniform microstructures will fail in the form of instantaneous implosion after being subjected to external pressure, which lacks safety during underwater work and is prone to accidents. Therefore, it is crucial to find a deep-sea pressure-resistant material with high elastic modulus, high compressive strength, and safety underwater. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a method for preparing an inorganic composite material, by changing the size matching of the raw material α-SiC particles and the amount of α-SiC fiber added, the material properties can be flexibly and conveniently adjusted. The microstructure of this inorganic composite material is uniform at the millimeter level and uneven at the micron level. The deep-sea pressure-resistant container made of this material is safe when working underwater.

[0006] The present invention solves the above technical problems through the following technical solutions:

[0007] The inorganic composite material of the invention consists of four physical phases: alpha-SiC, alpha-SiC fiber, beta-SiC and silicon phase.

[0008] The inorganic composite material of the present invention satisfies one or more of the following conditions:

[0009] The density of inorganic composite materials is 3.00-3.12g / cm 3 , for example, 3.05, 3.10 and 3.12 g / cm 3 ;

[0010] The compressive strength of the inorganic composite material is 3600-4000Mpa, for example, 3800, 3900, 4000Mpa;

[0011] The elastic modulus of the inorganic composite material is 390-410 GPa, for example, 395, 400 and 405 GPa;

[0012] The hardness of the inorganic composite material is HRA85-93, for example, HRA90, HRA92 and HRA93;

[0013] The fracture toughness of inorganic composite materials is 5-9MPa·m 1 / 2 , for example, 5, 7 and 9 MPa·m 1 / 2 ;

[0014] The inorganic composite material has a flexural strength of 330-420 MPa, for example, 350, 360 and 420 MPa.

[0015] The present invention also provides a method for preparing the above inorganic composite material, comprising the following steps:

[0016] S1, uniformly mixing α-SiC fiber, α-SiC particles and phenolic resin to obtain a slurry, and spray drying to obtain a spherical particle raw material;

[0017] Wherein, the length of α-SiC fiber is ≤300 μm and the diameter is ≤10 μm;

[0018] The particle size of α-SiC particles is 1-100 μm;

[0019] S2, pressing the spherical particle raw material into a green blank, and then curing the green blank;

[0020] S3, after the curing treatment, siliconizing treatment is performed.

[0021] In the present invention, α-SiC fibers are combined with α-SiC particles of different particle sizes to adjust the toughness, strength and rigidity of the material, which can effectively improve the performance of the material and solve the technical problem that secondary SiC is very easy to block the capillary channel, resulting in the incomplete sintering of the green billet.

[0022] The following further describes the parameters and conditions in step S1:

[0023] In the present invention, the feed ratio of α-SiC fiber, α-SiC particles and phenolic resin is (6-30):(60-84):10 in parts by weight.

[0024] In the present invention, preferably, the length of the α-SiC fiber is 100-300 μm, for example, 80% of the α-SiC fiber has a length of 200-300 μm, and 20% of the α-SiC fiber has a length of 100-200 μm;

[0025] Preferably, the particle size of the α-SiC particles is 1-15 μm, for example, the particle sizes of the α-SiC particles are 1, 5, and 15 μm, each accounting for 33.3%;

[0026] Alternatively, the particle size of the α-SiC particles is 10-50 μm, for example, the particle sizes of the α-SiC particles are 50, 20, and 10 μm, each accounting for 33.3%;

[0027] Alternatively, the particle size of the α-SiC particles is 10-100 μm, for example, the particle sizes of the α-SiC particles are 100, 60, and 10 μm, each accounting for 33.3%.

[0028] In the present invention, uniform mixing is achieved by ball milling in a stirred mill;

[0029] Preferably, the abrasive for ball milling is SiC ball or SiN ball, wherein the mass ratio of the abrasive to the raw material to be processed is 2:1;

[0030] Preferably, the rotation speed of the ball mill is 50-100 r / min, for example 70 r / min;

[0031] Preferably, the ball milling time is 3-5 hours, for example 5 hours;

[0032] Preferably, during the ball milling process, an auxiliary agent and water are also added, wherein the auxiliary agent includes one or more of a binder, a dispersant, a release agent and a lubricant;

[0033] Wherein, the binder is preferably polyvinyl alcohol or methyl cellulose, and the addition amount is 2-5% (relative to the mass percentage of the raw material);

[0034] Wherein, the dispersant is preferably polyacrylamide, and the addition amount is 2% (relative to the mass percentage of the raw material);

[0035] Wherein, the release agent is preferably a fatty alcohol or polysiloxane, and the addition amount is 2% (relative to the mass percentage of the raw material);

[0036] Wherein, the lubricant is preferably glycerol or dibutyl phthalate, and the addition amount is 1% (relative to the mass percentage of the raw material);

[0037] Preferably, the mass ratio of water to phenolic resin is 10:1.

[0038] In the present invention, a moisturizer may be added during the ball milling process according to the conventional practice in the art.

[0039] The following further describes the parameters and conditions in step S2:

[0040] In the present invention, the compression molding method is a molding method or an isostatic pressing method; wherein the molding method is a single-side pressing method or a double-side pressing method; the isostatic pressing method includes a dry bag isostatic pressing method or a wet bag isostatic pressing method;

[0041] Preferably, the pressure of the molding method or the isostatic pressing method is 120-150Mpa;

[0042] Preferably, the curing process is carried out in an oven;

[0043] Preferably, the curing treatment is to select 3-5 temperature values ​​in the range of 40°C-100°C and keep them warm for 1 to 5 hours respectively;

[0044] Preferably, the curing treatment is to heat to 60°C and keep warm for 3 hours, heat to 70°C and keep warm for 3 hours, heat to 100°C and keep warm for 3 hours; or, method two, heat to 40°C and keep warm for 3 hours, heat to 50°C and keep warm for 3 hours, heat to 60°C and keep warm for 3 hours, heat to 70°C and keep warm for 3 hours, heat to 100°C and keep warm for 3 hours; or, method three, heat to 50°C and keep warm for 3 hours, heat to 60°C and keep warm for 3 hours, heat to 70°C and keep warm for 3 hours, heat to 100°C and keep warm for 3 hours.

[0045] The following further describes the parameters and conditions in step S3:

[0046] In the present invention, the siliconizing treatment steps are as follows: adding silicon particles to the bottom of the vessel, placing the blank into the vessel, placing silicon particles on the surface of the blank, placing the vessel into a high-temperature kiln, evacuating the vessel, and then heating, keeping the temperature, and cooling the vessel;

[0047] Preferably, the particle size of the silicon particles is 0.05-2 mm;

[0048] Preferably, the vessel is a graphite crucible or a graphite plate;

[0049] Preferably, the vessel is sprayed with boron nitride powder before siliconizing treatment;

[0050] In the present invention, the container is sprayed with boron nitride powder before loading, which can prevent the silicon liquid or silicon vapor from reacting with the container and avoid silicon adhesion.

[0051] Preferably, in step S3, the vacuuming is stopped when the furnace temperature reaches 1450°C;

[0052] In the present invention, in step S3, the heating process satisfies one or more of the following conditions:

[0053] The heating process starts when the furnace vacuum drops to 1Pa;

[0054] The heating rate from room temperature to 900°C is 2-5°C / min, for example 2°C / min;

[0055] When the furnace temperature is from 900°C to 1450°C, the heating rate is 5-10°C / min, for example, 5°C / min;

[0056] The heating rate when the furnace temperature is from 1450 to 1650°C is 3°C / min;

[0057] The pressure is less than 10Pa during the heating process.

[0058] In the present invention, in step S3, the heat preservation process satisfies one or more of the following conditions:

[0059] Keep the temperature at 500℃, 750℃, 1000℃, 1450℃, 1700℃ for 1-2 hours;

[0060] When the furnace temperature is 1700℃, the insulation pressure is maintained at 30Pa.

[0061] In the present invention, in step S3, the cooling process satisfies one or more of the following conditions:

[0062] The cooling process is to reduce the furnace temperature from 1700°C to 1000°C, and then naturally cool to room temperature;

[0063] During the cooling process, the cooling rate from the furnace temperature of 1700°C to 1000°C is 5-10°C / min.

[0064] The present invention also provides an inorganic composite material prepared by using the preparation method of the inorganic composite material.

[0065] The present invention also provides the use of the above inorganic composite material in deep-sea pressure-resistant vessels;

[0066] Preferably, the above-mentioned inorganic composite material can be used in instrument cabins, deep-sea seismometers, detection shell containers, deep-sea buoyancy units, deep-sea landers, and deep-sea salvage buoyancy equipment.

[0067] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0068] The reagents and raw materials used in the present invention are commercially available.

[0069] The positive and progressive effects of the present invention are:

[0070] (1) The inorganic composite material of the present invention is composed of four phases, namely: α-SiC, α-SiC fiber, β-SiC and silicon phase, wherein β-SiC and silicon phase are newly generated connecting phases and gap filling phases. This microstructure improves the density and mechanical properties of the composite material. When used in deep-sea pressure-resistant vessels such as instrument cabins, the material has high compressive strength and high elastic modulus, which can reduce the thickness of the cabin wall and effectively increase the cabin loading capacity.

[0071] (2) The failure mode of the deep-sea pressure-resistant container made of the inorganic composite material of the present invention under pressure is the formation of cracks at both ends of the shell. When the pressure is continued to be increased, the cracks expand and water enters the shell. This phenomenon indicates that the failure mode is instability, and the cracks in the shell will not expand rapidly, so the safety is relatively high when working underwater.

[0072] (3) When the inorganic composite material of the present invention is used to manufacture large-sized spherical shells or cylindrical shells, the volume shrinkage from the green body to the completion of sintering is less than 1%, which means that the yield of large-sized spherical shells or cylindrical shells is extremely high, reaching more than 95%. BRIEF DESCRIPTION OF THE DRAWINGS

[0073] Figure 1 This is a SEM image of the fracture of the inorganic composite material obtained in Example 3 of the present invention;

[0074] Figure 2 This is a SEM image of the plane polishing of the inorganic composite material obtained in Example 3 of the present invention. DETAILED DESCRIPTION

[0075] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0076] In the sample performance test, the density is measured according to the national standard GB / T 3850-83 "Determination method of density of dense sintered metal materials and cemented carbides";

[0077] The compressive strength is measured in accordance with the national standard GB / T 8489-2006 "Test method for compressive strength of fine ceramics";

[0078] The elastic modulus is measured according to ISO_17561_2002(E) "Measurement of elastic modulus of bulk ceramics at room temperature by acoustic resonance method";

[0079] The hardness is measured in accordance with the national standard GB / T 16534 "Vickers hardness test method for engineering ceramics";

[0080] The fracture toughness was measured according to ISO_15732_2003(E) “Fracture toughness of bulk ceramics at room temperature by single-edge notched beam (SEPB) method”;

[0081] The flexural strength is measured in accordance with the national standard GB / T 6569-2006 "Test method for flexural strength of fine ceramics";

[0082] The Weibull modulus is used to reflect the discreteness of material strength. The higher the Weibull modulus, the smaller the discreteness. In the present invention, the Weibull modulus is measured according to ISO_20501_2003 "Weibull Statistics of Fine Ceramics Strength Data".

[0083] Example 1

[0084] α-SiC fibers (80% of which have a fiber length of 200-300 μm, 20% of which have a fiber length of 100-200 μm, and a diameter of ≤10 μm), α-SiC particles (D50 = 15, 5, 1 μm, 33.3% each), and phenolic resin were weighed at 25, 65, and 10 kg, respectively. 100 kg of water was first put into a stirred mill, and SiC balls or SiN balls were added, wherein the mass ratio of the abrasive to the raw material to be processed was 2:1, and then 2% of the polyol was added in sequence. Acrylamide, α-SiC fiber, α-SiC particles, and phenolic resin are mixed at a speed of 70 r / min for 5 hours, during which 5% methyl cellulose, 1% dibutyl phthalate, and 2% polysiloxane are added, and the slurry is spray-dried to obtain a mixed spherical particle raw material; the prepared raw materials are filled into a blank mold, and a double-sided press is used to press the blank at a pressure of 120 MPa; the pressed blank is placed in an oven for curing, and the temperature is raised to 40°C for 3 hours, and the temperature is raised to 50°C for 3 hours. The solidified green billet is placed in a graphite crucible sprayed with boron nitride powder, silicon particles with a particle size of 0.05-2 mm are placed on the upper and lower parts of the green billet, and the weight of the silicon particles is equivalent to the weight of the green billet. The graphite crucible is placed in a kiln and vacuum is started. When the vacuum degree of the furnace body is reduced to 1 Pa, heating is started; the heating rate is 3°C / min from room temperature to 900°C, and 900- The heating rate to 1450℃ is 6℃ / min, and the heating rate to 1450-1650℃ is 3℃ / min; when the furnace temperature reaches 1450℃, stop vacuuming, and the pressure is less than 10Pa during the infiltration process; keep warm for 1 hour at 500, 750, 1000, 1450, and 1700℃ respectively; the pressure is maintained at 30Pa when keeping warm at 1700℃; during the cooling process, the cooling rate at 1700-1000℃ is 5℃ / min, and it cools to room temperature with the furnace when reaching 1000℃.

[0085] After the blank is taken out of the furnace, it is sandblasted to remove the excess silicon on the surface; the blank is cut and made into test samples. The test results are: Density: 3.12g / cm 3 , compressive strength: 3900Mpa, elastic modulus: 400Gpa, hardness: HRA93, fracture toughness: 9MPa·m 1 / 2 , Flexural strength: 420Mpa (Weibull modulus of flexural strength is greater than 5).

[0086] Example 2

[0087] α-SiC fibers (80% of which have a fiber length of 200-300 μm, 20% of which have a fiber length of 100-200 μm, and a diameter of ≤10 μm), α-SiC particles (D50 = 50, 20, 10 μm, 33.3% each), and phenolic resin were weighed at 15, 75, and 10 kg, respectively. 100 kg of water was first put into a stirred mill, and SiC balls or SiN balls were added, wherein the mass ratio of the abrasive to the raw material to be processed was 2:1, and then 2% of Polyacrylamide, α-SiC fiber, α-SiC particles, and phenolic resin are mixed at a speed of 70r / min for 5 hours, during which 2% polyvinyl alcohol, 1% glycerol, and 2% fatty alcohol are added, and the slurry is spray-dried to obtain a mixed spherical particle raw material; the green blank mold is filled with the prepared raw materials, and is placed in a wet bag isostatically pressed rubber and plastic soft film, and pressed at a pressure of 150MPa to obtain an isotropic high-quality green blank; the pressed green blank is placed in an oven for curing, and the temperature is raised to 50 ℃ and keep warm for 3 hours, then heat up to 60℃ and keep warm for 3 hours, then heat up to 70℃ and keep warm for 3 hours, then heat up to 100℃ and keep warm for 3 hours; put the solidified green billet into a graphite crucible sprayed with boron nitride powder, and place silicon particles with a particle size of 0.05-2mm on the top and bottom of the green billet. The weight of the silicon particles is equivalent to the weight of the green billet. Put the graphite crucible into the kiln and start evacuating. When the vacuum degree of the furnace body is reduced to 1Pa, start heating; the heating rate is 3℃ / min from room temperature to 900℃, 900 The heating rate from -1450℃ is 6℃ / min, and the heating rate from 1450-1650℃ is 3℃ / min; when the furnace temperature reaches 1450℃, stop evacuating, and the pressure is less than 10Pa during the infiltration process; keep warm for 1 hour at 500, 750, 1000, 1450, and 1700℃ respectively; when keeping warm at 1700℃, the pressure is maintained at 30Pa; during the cooling process, the cooling rate is 5℃ / min at 1700-1000℃, and cool to room temperature with the furnace when reaching 1000℃.

[0088] After the blank is taken out of the furnace, it is sandblasted to remove the excess silicon on the surface; the blank is cut and made into test samples. The test results are: Density: 3.10g / cm 3 , compressive strength: 4000Mpa, elastic modulus: 395Gpa, hardness: HRA92, fracture toughness: 7MPa·m 1 / 2 , Flexural strength: 360Mpa (Weibull modulus of flexural strength is greater than 7).

[0089] Example 3

[0090] α-SiC fibers (80% of which have a fiber length of 200-300 μm, 20% of which have a fiber length of 100-200 μm, and a diameter of ≤10 μm), α-SiC particles (D50 = 100, 60, 10 μm, 33.3% each), and phenolic resin are weighed at 36, 504, and 60 kg, respectively. First, 600 kg of water is put into a stirred mill, and SiC balls or SiN balls are added, wherein the mass ratio of the abrasive to the raw material to be processed is 2:1, and then the abrasive is mixed with the raw material to be processed. 2% polyacrylamide, α-SiC fiber, α-SiC particles, and phenolic resin were added, and mixed at a speed of 70 r / min for 5 hours. During this period, 2% polyvinyl alcohol, 1% glycerol, and 2% fatty alcohol were added, and the slurry was spray-dried to obtain a mixed spherical particle raw material; the prepared raw material was put into a dry bag isostatically pressed rubber and plastic soft film, and pressed at a pressure of 120 MPa to obtain an isotropic high-quality blank; the pressed blank was placed in an oven for curing, and the temperature was raised to 6 Keep the temperature at 0℃ for 3 hours, heat to 70℃ and keep it for 3 hours, heat to 100℃ and keep it for 3 hours; put the solidified blank into a graphite crucible sprayed with boron nitride powder, place silicon particles with a particle size of 0.05-2mm on the top and bottom of the blank, and the weight of the silicon particles is equivalent to the weight of the blank. Put the graphite crucible into the kiln and start evacuating. When the vacuum degree of the furnace body is reduced to 1Pa, start heating; the heating rate is 2℃ / min from room temperature to 900℃, and the heating rate is 900-1450℃. The speed is 5℃ / min, and the heating speed from 1450-1650℃ is 3℃ / min; when the furnace temperature reaches 1450℃, stop vacuuming, and the pressure during the infiltration process is less than 10Pa; keep warm at 500, 750, 1000, and 1450℃ for 1 hour each, and keep warm at 1700℃ for 2 hours; the pressure is maintained at 30Pa when keeping warm at 1700℃; during the cooling process, the cooling speed is 5℃ / min at 1700-1000℃, and it cools to room temperature with the furnace when it reaches 1000℃.

[0091] After the blank is taken out of the furnace, it is sandblasted to remove the excess silicon on the surface; the blank is cut and made into test samples. The test results are: Density: 3.05g / cm 3 , compressive strength: 3800MPa, elastic modulus: 405GPa, hardness: HRA90, fracture toughness: 5MPa·m 1 / 2 , Flexural strength: 350Mpa (Weibull modulus of flexural strength is greater than 8).

[0092] Figure 1 This is a SEM image of the fracture of the inorganic composite material obtained in Example 3 of the present invention. As can be seen from the figure, the inorganic composite material obtained in Example 3 of the present invention is composed of four phases: α-SiC, α-SiC fiber, β-SiC and silicon phase, among which β-SiC and silicon phase are newly generated connecting phases and gap filling phases, and the material is uneven at the micron level.

[0093] Figure 2 This is a SEM image of the plane polishing of the inorganic composite material obtained in Example 3 of the present invention. As can be seen from the image, the inorganic composite material obtained in Example 3 of the present invention is uniform on the millimeter scale.

[0094] Application Example 1

[0095] According to Example 3, during the process of pressing the green billet, the prepared powder raw material is placed in a dry bag isostatically pressed cylindrical or hemispherical shell rubber and plastic soft film, and finally a pressure-resistant cylinder and a cylinder head hemispherical shell with an outer diameter of 300 (length 800), 500 (length 1200), and 900 (length 1500) mm are obtained, respectively. The finished product rate of the pressure-resistant cylinder is 95%, and the finished product rate of the cylinder head hemispherical shell is 100%. The volume shrinkage rate of the two products from the green body to the completion of sintering is ≤1%.

[0096] The ground pressure test was carried out by simulating the deep sea depths of 11000 meters, 7000 meters and 4000 meters. The pressure test of 115MPa was carried out on the three outer diameter composite pressure hulls respectively, and the fatigue failure test was carried out. The results show that the compressive strength of the composite pressure hull increases with the increase of the shell wall thickness. The shell with an outer diameter of 300mm and a wall thickness of 13mm can be cyclically depressurized and pressurized 10 times under a pressure of 115MPa; the shell with an outer diameter of 500mm and a wall thickness of 18mm can be cyclically depressurized and pressurized 5 times under a pressure of 75MPa; the shell with an outer diameter of 900mm and a wall thickness of 30mm can be cyclically depressurized and pressurized 3 times under a pressure of 50MPa. The failure form under pressure is the formation of cracks at both ends of the shell. If the pressure is continued, the cracks will expand and water will enter the shell. This phenomenon indicates that the failure form is instability. The analysis of the composite material after failure shows that the microstructure of the material is uneven (in the range of 0.1-100μm), and the cracks will not expand rapidly. Among them, α-SiC fibers and large-sized α-SiC particles play a role in preventing crack propagation.

[0097] Application Example 2

[0098] The samples of Example 1-2 were tested with reference to Application Example 1, and the data obtained showed the same result: the compressive strength of the composite pressure-resistant shell of Example 1-2 increases with the increase of the shell wall thickness. The shell with an outer diameter of 300mm and a wall thickness of 13mm can be cyclically depressurized and pressurized 10 times at a pressure of 115MPa; the shell with an outer diameter of 500mm and a wall thickness of 18mm can be cyclically depressurized and pressurized 5 times at a pressure of 75MPa; the shell with an outer diameter of 900mm and a wall thickness of 30mm can be cyclically depressurized and pressurized 3 times at a pressure of 50MPa.

Claims

1. An inorganic composite material, characterized in that: It consists of four phases: α-SiC, α-SiC fiber, β-SiC and silicon phase.

2. The inorganic composite material according to claim 1, characterized in that The inorganic composite material meets one or more of the following conditions: The density of the inorganic composite material is 3.00-3.12 g / cm 3 , for example, 3.05, 3.10 and 3.12 g / cm 3 ; The compressive strength of the inorganic composite material is 3600-4000 MPa, for example, 3800, 3900, 4000 MPa; The elastic modulus of the inorganic composite material is 390-410 GPa, for example, 395, 400 and 405 GPa; The hardness of the inorganic composite material is HRA85-93, for example, HRA90, HRA92 and HRA93; The fracture toughness of the inorganic composite material is 5-9 MPa·m 1 / 2 , for example, 5, 7 and 9 MPa·m 1 / 2 ; The flexural strength of the inorganic composite material is 330-420 MPa, for example, 350, 360 and 420 MPa.

3. A method for preparing an inorganic composite material, characterized in that: It includes the following steps: S1, uniformly mixing α-SiC fiber, α-SiC particles and phenolic resin to obtain a slurry, and spray drying to obtain a spherical particle raw material; Wherein, the length of the α-SiC fiber is ≤300 μm and the diameter is ≤10 μm; The particle size of the α-SiC particles is 1-100 μm; S2, pressing the spherical particle raw material into a green blank, and then curing the green blank; S3, performing siliconizing treatment after the curing treatment.

4. The preparation method according to claim 3, characterized in that: In step S1, the feed ratio of α-SiC fiber, α-SiC particles and phenolic resin is (6-30):(60-84):10 in parts by weight.

5. The preparation method according to claim 3, characterized in that: In step S1, the length of the α-SiC fibers is 100-300 μm, for example, 80% of the α-SiC fibers are 200-300 μm in length, and 20% of the α-SiC fibers are 100-200 μm in length; And / or, the particle size of the α-SiC particles is 1-15 μm, for example, the particle sizes of the α-SiC particles are 1, 5, and 15 μm, each accounting for 33.3%; Alternatively, the particle size of the α-SiC particles is 10-50 μm, for example, the particle sizes of the α-SiC particles are 50, 20, and 10 μm, each accounting for 33.3%; Alternatively, the particle size of the α-SiC particles is 10-100 μm. For example, the particle sizes of the α-SiC particles are 100, 60, and 10 μm, each accounting for 33.3%.

6. The preparation method according to claim 3, characterized in that: In step S1, the uniform mixing is achieved by ball milling in a stirred mill; Preferably, the abrasive of the ball mill is SiC ball or SiN ball, wherein the mass ratio of the abrasive to the raw material to be processed is 2:1; And / or, the rotation speed of the ball mill is 50-100 r / min, for example 70 r / min; And / or, the ball milling time is 3-5 hours, for example 5 hours; And / or, during the ball milling process, an auxiliary agent and water are further added, wherein the auxiliary agent includes one or more of a binder, a dispersant, a release agent and a lubricant; Preferably, the binder is polyvinyl alcohol or methyl cellulose, and the addition amount is 2-5%, where the % is the mass percentage relative to the raw material; Preferably, the dispersant is polyacrylamide, and the addition amount is 2%, where the % is the mass percentage relative to the raw material; Preferably, the release agent is fatty alcohol or polysiloxane, and the addition amount is 2%, where the % is the mass percentage relative to the raw material; Preferably, the lubricant is glycerol or dibutyl phthalate, and the added amount is 1%, where the % is the mass percentage relative to the raw material; Preferably, the mass ratio of the water to the phenolic resin is 10:

1.

7. The preparation method according to claim 3, characterized in that: Step S2 satisfies one or more of the following conditions: The compression molding method is a molding method or an isostatic pressing method; wherein the molding method is a single-side pressing method or a double-side pressing method; and the isostatic pressing method is a dry bag isostatic pressing method or a wet bag isostatic pressing method; Preferably, the pressure of the molding method or isostatic pressing method is 120-150Mpa; And / or, the curing process is carried out in an oven; And / or, the curing treatment is to select 3 to 5 temperature values ​​within the range of 40° C. to 100° C. and keep them warm for 1 to 5 hours respectively; Preferably, method 1 is used, and the curing treatment is to heat the temperature to 60°C and keep it for 3 hours, heat the temperature to 70°C and keep it for 3 hours, and heat the temperature to 100°C and keep it for 3 hours; or, method 2 is to heat the temperature to 40°C and keep it for 3 hours, heat the temperature to 50°C and keep it for 3 hours, heat the temperature to 60°C and keep it for 3 hours, heat the temperature to 70°C and keep it for 3 hours, and heat the temperature to 100°C and keep it for 3 hours; or, method 3 is to heat the temperature to 50°C and keep it for 3 hours, heat the temperature to 60°C and keep it for 3 hours, heat the temperature to 70°C and keep it for 3 hours, and heat the temperature to 100°C and keep it for 3 hours.

8. The preparation method according to claim 3, characterized in that: In step S3, the siliconizing treatment step is to add silicon particles to the bottom of the vessel, put the blank into the vessel, and also place silicon particles on the surface of the blank, put the vessel into a high-temperature kiln to evacuate, and then heat, keep warm and cool down; Wherein, the particle size of the silicon particles is 0.05-2 mm; The vessel is a graphite crucible or a graphite plate; And / or, the vessel is sprayed with boron nitride powder before the siliconizing treatment; And / or, the vacuuming is stopped when the furnace temperature reaches 1450°C; And / or, during the heating process, one or more of the following conditions are met: The heating process starts when the vacuum degree of the furnace body drops to 1 Pa; During the heating process, the heating rate is 2-5°C / min, for example 2°C / min, when the furnace temperature is from room temperature to 900°C. During the heating process, when the furnace temperature is from 900°C to 1450°C, the heating rate is 5-10°C / min, for example, 5°C / min; During the heating process, the heating rate is 3°C / min when the furnace temperature is from 1450 to 1650°C; During the heating process, the pressure is less than 10 Pa; And / or, during the heat preservation process, one or more of the following conditions are met: During the heat preservation process, the furnace temperature is kept at 500° C., 750° C., 1000° C., 1450° C., and 1700° C. for 1-2 hours; During the heat preservation process, the pressure is maintained at 30 Pa when the furnace temperature is 1700°C; And / or, during the cooling process, one or more of the following conditions are met: During the cooling process, after the furnace temperature is reduced from 1700°C to 1000°C, it is naturally cooled to room temperature; During the cooling process, the cooling rate from the furnace temperature of 1700° C. to 1000° C. is 5-10° C. / min.

9. An inorganic composite material obtained by the preparation method according to any one of claims 3 to 8.

10. An application of the inorganic composite material as described in any one of claims 1, 2 or 9 in a deep-sea pressure-resistant container, wherein the deep-sea pressure-resistant container is preferably any one of the following containers: an instrument cabin, a deep-sea seismograph, a detection shell container, a deep-sea buoyancy unit, a deep-sea lander, and a deep-sea salvage buoyancy equipment.

Citation Information

Patent Citations

  • Reactive sintering siliconcarbide ceramics preparation method taking mesocarbon microbead (MCMB) as carbon source

    CN101747044A

  • High-performance low-free-silicon-content reactive sintering silicon carbide ceramic material and preparation method thereof

    CN115057707A

  • Reaction-sintered ceramic and process for producing the same

    CN1157276A

  • Sleeving structure of SiC fiber reinforced metal matrix composite variable-diameter pipe shaft part and precursor wire laying method