Light-weight high-strength ceramsite based on phosphate tailings as well as preparation method and application of light-weight high-strength ceramsite

By optimizing the sintering process of phosphorus tailings combination raw materials, lightweight and high-strength ceramic granules were prepared, which solved the problem of low utilization rate of phosphorus tailings resources and difficult to take into account both the performance of ceramic granules, and achieved efficient utilization of phosphorus tailings resources and ceramic granules. promote.

CN118930304APending Publication Date: 2024-11-12WUHAN UNIV OF SCI & TECH +1

Patent Information

Application Number
CN202411067472.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The low utilization rate of existing phosphorus tailings resources leads to waste of resources and environmental pollution. The lightweight and high-strength performance of the ceramic granules are difficult to take into account, the process is complex and the cost is high.

Method used

Combination raw materials are used for 61 to 76 parts of siliceous phosphorus tailings, 14 to 19 parts of steel slag, 5 to 10 parts of fluorite tailings, 5 to 10 parts of water-washed secondary aluminum ash, 3 to 5 parts of dextrin and 3 to 5 parts of activated carbon. , lightweight high-strength ceramic granules are prepared through granulation, drying, preheating and sintering processes, optimized sintering temperature and time, and formed a multi-porous structure to improve strength and reduce density.

Benefits of technology

It realizes lightweight and high-strength performance coordination of ceramic particles, with a volume density of 1100~1400kg/m3, a cylinder pressure strength of 13.5~16.1MPa, a heavy metal curing rate of 95%, a simple process and low cost, and is suitable for lightweight concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004980580640000131
    Figure BDA0004980580640000131
Patent Text Reader

Abstract

The invention relates to the technical field of comprehensive utilization of phosphate tailing resources, and discloses light-weight high-strength ceramsite based on phosphate tailings as well as a preparation method and application of the light-weight high-strength ceramsite. The lightweight high-strength ceramsite is prepared from the following raw materials in parts by mass: 61-76 parts of siliceous phosphate tailings, 14-19 parts of steel slag, 5-10 parts of fluorite tailings, 5-10 parts of washed secondary aluminum ash, 3-5 parts of dextrin, 3-5 parts of activated carbon and 5-9 parts of water. According to the light-weight high-strength ceramsite based on the phosphate tailings, the volume density is 1100-1400 kg / m < 3 >, the cylinder compressive strength is 13.5-16.1 MPa, the stacking density is 550-670 kg / m < 3 >, the water absorption rate is 3-9%, the curing rate of heavy metal ions reaches 95% or above, safe use of light-weight concrete can be achieved, all the adopted raw materials are solid waste, comprehensive utilization of the phosphate tailings resources is fully achieved, and the light-weight high-strength ceramsite based on the phosphate tailings is suitable for industrial production. The recycling rate is high and the production cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of comprehensive utilization of phosphorus tailings resources, and in particular to a lightweight and high-strength ceramsite based on phosphorus tailings, and a preparation method and application thereof. Background Art

[0002] In the current production practice of ceramsite, the raw materials mainly come from natural resources such as clay and shale, while the research on the production of ceramsite using solid waste is still insufficient. Over-reliance on clay and shale as raw materials not only leads to the consumption of natural resources, but also faces the problem of production restrictions due to the implementation of the "ban on clay" policy. Therefore, converting solid waste into raw materials for the production of ceramsite has become a preferred choice, which not only helps to reduce production costs, but also promotes the value-added utilization of solid waste. Take phosphate tailings as an example, which is the solid waste generated after the enrichment of P2O5 in the phosphate ore beneficiation process. According to the "China Mineral Resources Report", as of 2022, the stockpile of phosphate tailings in my country will be about 1.2 billion tons, and it will grow at a rate of 15% per year. The long-term stacking of such a large amount of phosphate tailings not only occupies a large amount of land resources, but also may lead to serious vegetation damage, heavy metal leakage and pollution of groundwater sources, and the safety risk of tailings dam collapse.

[0003] At present, the research on phosphorus tailings resources mainly focuses on the recovery of phosphorus, the extraction of rare metals and rare earth elements, and the comprehensive utilization of silicates. However, the utilization rate of these methods still needs to be improved. The large accumulation of phosphorus tailings not only brings huge challenges to the mining industry, the economy and the environment, but also causes serious waste of resources. In order to solve the problems of large accumulation of phosphorus tailings, less tailings raw materials used in the preparation of ceramsite and complex processes, technicians have conducted in-depth research and technical development:

[0004] For example, Chinese invention patent CN106747600A discloses a sintered ceramsite and method using phosphorus tailings as the main raw material, which discloses a method of wet grinding 40-50 parts of phosphorus tailings and 20-35 parts of steel slag, adding 10-20 parts of fly ash, and then adding 30-40 parts of water to obtain a slurry, and the slurry is added with a binder and carbon powder to obtain a raw material ball in a granulator, and then placed in a drying box for drying after natural drying, and then preheated in a rotary kiln preheating zone, and then placed in a rotary kiln high temperature zone for calcination, and cooled to room temperature to obtain sintered ceramsite. Although the prepared ceramsite uses phosphorus tailings as the main raw material, the proportion of phosphorus tailings is only 40-50 parts, and the phosphorus tailings resources cannot be fully utilized. In addition, although the wet grinding of the prepared ceramsite fully stimulates the potential activity of the raw materials and avoids dust pollution caused by drying and dry grinding, it still needs room temperature drying, drying oven drying, rotary kiln preheating, and rotary kiln high temperature zone calcination after wet grinding. The operation process is complicated, the production cycle is long, and the cost is high. Finally, the compressive strength of ceramsite is 26.83-28.63MPa, but the density of ceramsite is large, so it can only be used to configure high-strength concrete. It cannot meet the demand for lightweight building materials required for high-rise and large-span buildings today, nor can it achieve the synergy of the two properties of lightweight and high strength of ceramsite.

[0005] Another Chinese invention patent CN114394850A discloses a high-performance ceramsite based on phosphate tailings and its preparation method. It discloses a method of using 80-95 parts of high-silicon phosphate tailings and 5-20 parts of high-magnesium-calcium phosphate tailings as raw materials, adding 3-5 parts of dextrin, mixing and placing in a granulator, spraying 2-5 parts of a 3% polyvinyl alcohol aqueous solution, drying after granulation; sintering in a medium-temperature furnace and cooling with the furnace; then placing in a modified solution, oscillating in a constant temperature oscillator, standing, and drying to obtain high-performance ceramsite based on phosphate tailings. The bulk density of the ceramsite is 0.7-1.1 g / cm 3 However, the strength is only 5-7MPa, which cannot meet the demand for high-strength building materials required for today's high-rise and large-span buildings, nor can it achieve the synergy of the lightweight and high-strength properties of expanded clay.

[0006] Another Chinese invention patent CN116102359A discloses a lightweight and high-strength ceramsite and its preparation method, which discloses a method of preparing ceramsite by granulating 62-68 parts of coal-based solid waste, 10-15 parts of modified attapulgite, 12-16 parts of modified corn cobs, 4-6 parts of microsilica powder, 10-13 parts of binder, 2-3 parts of cement-based adhesive and 1-2 parts of plasticizer. Although the prepared ceramsite has the characteristics of light weight and high strength (its bulk density can be as low as 418kg / m 3, the cylinder pressure strength can be as high as 10MPa or more). Although the synergy of the two properties of light weight and high strength of expanded clay is achieved, the raw materials need to be processed: the attapulgite must be calcined, and then dodecyltriphenylphosphonium bromide, hexadecyltrimethylammonium bromide and water are added, and the modified attapulgite is obtained after reaction, filtration and drying; the corn cob must first be heated by microwave, and then soaked in a sodium bicarbonate aqueous solution to obtain the modified corn cob; the operating process for preparing expanded clay is complicated, the production cycle is long, and the production cost is high; and the maximum cylinder pressure strength of expanded clay is only 11.2MPa.

[0007] Therefore, it is of great significance to study the preparation method and application of expanded clay that can simultaneously meet the conditions of green environmental protection and simple process, and can solve the synergistic problems of light weight and high strength. Summary of the invention

[0008] In view of this, the present invention provides a lightweight and high-strength ceramsite based on phosphate tailings and a preparation method and application thereof, so that it can solve the problem that the existing lightweight and high-strength properties of ceramsite cannot be coordinated or can be coordinated but the process is complicated and the cost is high. At the same time, it solves the problem of serious waste of resources and great impact on mining, economy and environment caused by excessive stockpiles of existing phosphate tailings.

[0009] In order to achieve the above object, the present invention adopts the following technical solution:

[0010] The present invention provides a lightweight and high-strength ceramsite based on phosphate tailings, which is prepared from the following raw materials in parts by weight:

[0011] 61-76 parts of siliceous phosphorus tailings, 14-19 parts of steel slag, 5-10 parts of fluorite tailings, 5-10 parts of washed secondary aluminum ash, 3-5 parts of dextrin, 3-5 parts of activated carbon and 5-9 parts of water.

[0012] Preferably, the silicon dioxide content in the siliceous phosphate tailings is ≥57wt%, and the particle size of the siliceous phosphate tailings is ≤74μm.

[0013] Preferably, the sum of the contents of calcium oxide and magnesium oxide in the steel slag is ≥50wt%, and the particle size of the steel slag is ≤74μm.

[0014] Preferably, the silicon dioxide content in the fluorite tailings is ≥70wt%, and the particle size of the fluorite tailings is ≤74μm.

[0015] Preferably, the aluminum oxide content in the water-washed secondary aluminum ash is ≥68wt%, and the particle size of the water-washed secondary aluminum ash is ≤74μm.

[0016] Preferably, the purity of the dextrin is ≥99%, and the particle size of the dextrin is ≤8 μm; the purity of the activated carbon is ≥99%, and the particle size of the activated carbon is ≤8 μm.

[0017] The present invention also provides a method for preparing the lightweight and high-strength ceramsite based on phosphate tailings, which is characterized by comprising the following steps:

[0018] Siliceous phosphate tailings, steel slag, fluorite tailings, washed secondary aluminum ash, dextrin, activated carbon and water are mixed and then granulated, dried, preheated and sintered in sequence to obtain lightweight and high-strength ceramsite based on phosphate tailings.

[0019] Preferably, the drying temperature is 100-110° C., and the drying time is 24-32 hours.

[0020] Preferably, the preheating temperature is 800-900°C, the preheating time is 10-30 min, the sintering temperature is 1110-1200°C, the sintering time is 0.5-3 h, the heating rate from room temperature to the preheating temperature is 1-2°C / min, and the heating rate from the preheating temperature to the sintering temperature is 1-2°C / min.

[0021] The present invention also provides application of the lightweight high-strength ceramsite based on phosphate tailings in lightweight concrete.

[0022] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) The lightweight high-strength ceramsite based on phosphate tailings prepared in the present invention has a bulk density of 1100 to 1400 kg / m 3 , cylinder pressure strength 13.5~16.1MPa, bulk density 550~670kg / m 3 , water absorption rate is 3-9%, and the solidification rate of heavy metal ions is more than 95%; the prepared lightweight and high-strength ceramsite has a microporous structure inside, and because of its advantages of high strength, low density and strong practicality, it can solve the problem that the existing ceramsite cannot have both lightweight and high strength properties, or has both lightweight and high strength properties but has a complex preparation process and high cost.

[0024] (2) The raw materials used in the present invention are all solid waste, which fully realizes the comprehensive utilization of phosphorus tailings resources. At the same time, it solves the problem of serious waste of resources and great impact on mining, economy and environment caused by excessive stockpiles of existing phosphorus tailings. It can be safely used in lightweight concrete. The preparation method of the present invention has the characteristics of high utilization rate of phosphorus tailings resources, simple process, low production cost and short production cycle. DETAILED DESCRIPTION

[0025] The present invention provides a lightweight and high-strength ceramsite based on phosphate tailings, which is prepared from the following raw materials in parts by weight:

[0026] 61-76 parts of siliceous phosphorus tailings, 14-19 parts of steel slag, 5-10 parts of fluorite tailings, 5-10 parts of washed secondary aluminum ash, 3-5 parts of dextrin, 3-5 parts of activated carbon and 5-9 parts of water.

[0027] In the present invention, the amount of the siliceous phosphate tailings is preferably 62 to 73 parts, more preferably 64 to 70 parts, and more preferably 65 to 68 parts. The amount of the steel slag is preferably 15 to 18 parts, and more preferably 16 to 17 parts. The amount of the fluorite tailings is preferably 6 to 9 parts, and more preferably 7 to 8 parts. The amount of the water-washed secondary aluminum ash is preferably 6 to 9 parts, and more preferably 7 to 8 parts. The amount of dextrin is preferably 4 parts, the amount of activated carbon is preferably 4 parts, and the amount of water is preferably 6 to 8 parts, and more preferably 7 parts.

[0028] The silicon dioxide content in the siliceous phosphate tailings of the present invention is preferably ≥57wt%, further preferably ≥58wt%, more preferably ≥63wt%, and the particle size of the siliceous phosphate tailings is preferably ≤74μm, further preferably ≤68μm, more preferably ≤62μm.

[0029] The sum of the contents of calcium oxide and magnesium oxide in the steel slag of the present invention is preferably ≥50wt%, further preferably ≥58wt%, more preferably ≥62wt%, and the particle size of the steel slag is preferably ≤74μm, further preferably ≤68μm, more preferably ≤62μm.

[0030] The silicon dioxide content in the fluorite tailings of the present invention is preferably ≥70wt%, more preferably ≥76wt%, more preferably ≥83wt%, and the particle size of the fluorite tailings is preferably ≤74μm, more preferably ≤68μm, more preferably ≤62μm.

[0031] The content of alumina in the water-washed secondary aluminum ash of the present invention is preferably ≥68wt%, further preferably ≥74wt%, more preferably ≥78wt%, and the particle size of the water-washed secondary aluminum ash is preferably ≤74μm, further preferably ≤68μm, more preferably ≤62μm.

[0032] The purity of the dextrin of the present invention is preferably ≥99%, more preferably ≥99.9%, and more preferably ≥99.99%. The particle size of the dextrin is preferably ≤8 μm, more preferably ≤6 μm, and more preferably ≤4 μm.

[0033] The purity of the activated carbon of the present invention is preferably ≥99%, more preferably ≥99.9%, and more preferably ≥99.99%. The particle size of the activated carbon is preferably ≤8 μm, more preferably ≤6 μm, and more preferably ≤4 μm.

[0034] The present invention also provides a method for preparing the lightweight and high-strength ceramsite based on phosphate tailings, which is characterized by comprising the following steps:

[0035] Siliceous phosphate tailings, steel slag, fluorite tailings, washed secondary aluminum ash, dextrin, activated carbon and water are mixed and then granulated, dried, preheated and sintered in sequence to obtain lightweight and high-strength ceramsite based on phosphate tailings.

[0036] In the preparation method described in the present invention, siliceous phosphate tailings, steel slag, fluorite tailings and washed secondary aluminum ash are preferably mixed, ground and dried once, and then dextrin and activated carbon are added to obtain a mixture, and then water is added to the mixture for granulation to obtain spherical particles, and the obtained spherical particles are sequentially dried, preheated and sintered to obtain lightweight and high-strength ceramsite based on phosphate tailings.

[0037] In the present invention, the washed secondary aluminum ash is secondary aluminum ash that has been treated with water, and the specific treatment method of the water washing treatment is: washing, filtering and drying the secondary aluminum ash in sequence; wherein, the particle size of the secondary aluminum ash is preferably ≤212μm, more preferably ≤200μm, and more preferably ≤190μm. During the water washing, the mass ratio of secondary aluminum ash to water is preferably 1:4-7, more preferably 1:5-6, the water washing time is preferably 15-30min, more preferably 20-28min, and more preferably 22-25min. The drying temperature is preferably 100-120°C, more preferably 103-115°C, and more preferably 108-110°C. The drying time is preferably 22-26h, more preferably 23-25h, and more preferably 24h.

[0038] In the present invention, the water washing treatment of the secondary aluminum ash can prevent the aluminum nitride therein from reacting with water at room temperature to generate toxic and harmful ammonia with a strong irritating odor, thereby avoiding environmental pollution and affecting human health.

[0039] In the present invention, the particle size of the ground powder is preferably 180-210 mesh, more preferably 185-200 mesh, and even more preferably 190-195 mesh.

[0040] In the present invention, the primary drying temperature is preferably 100-120°C, more preferably 105-115°C, more preferably 108-110°C, and the primary drying time is preferably 20-26h, more preferably 21-25h, more preferably 22-24h.

[0041] In the present invention, the secondary drying temperature is preferably 100-110°C, more preferably 102-108°C, more preferably 104-106°C, and the secondary drying time is preferably 24-32h, more preferably 25-30h, more preferably 26-28h.

[0042] In the present invention, the preheating temperature is preferably 800-900°C, more preferably 820-880°C, more preferably 840-860°C, the preheating time is preferably 10-30min, more preferably 15-25min, more preferably 18-20min, the sintering temperature is preferably 1110-1200°C, more preferably 1120-1180°C, more preferably 1140-1160°C, the sintering time is preferably 0.5-3h, more preferably 1-2.5h, more preferably 1.5-2h, the heating rate from room temperature to the preheating temperature is preferably 1-2°C / min, more preferably 1.2-1.8°C / min, more preferably 1.4-1.6°C / min, and the heating rate from the preheating temperature to the sintering temperature is preferably 1-2°C / min, more preferably 1.2-1.8°C / min, more preferably 1.4-1.6°C / min.

[0043] In the present invention, (1) the raw materials used in the present invention can effectively improve the strength of ceramsite: in the medium-temperature heating stage (900-1100°C) of the siliceous phosphorus tailings and steel slag, amorphous Al2O3 and SiO2 begin to form amorphous aluminosilicate, i.e., the precursor of mullite; in the high-temperature heating stage (greater than 1100°C), the amorphous aluminosilicate forms mullite through the reaction of formula I.

[0044] In the present invention, the formula I is a solid-state reaction involving the rearrangement of Al and Si atoms to form mullite with a specific crystal structure. After being sintered at a high temperature for a period of time, the mullite crystals can continue to grow to form a larger crystal structure, thereby improving the strength of the ceramsite.

[0045] 3Al2O3+2SiO2→3Al2O3·2SiO2 Formula I

[0046] The steel slag of the present invention contains 26% Fe2O3. In the aluminosilicate-based system (i.e., the system described in Formula I), iron is used as a mineralizer to support the growth of mullite. Ceramsite with a high content of mullite crystals is obtained by sintering iron-rich materials and siliceous phosphorus tailings, thereby improving the strength of the ceramsite.

[0047] In the present invention, the main component of the washed secondary aluminum ash is corundum (Al2O3). At high temperature, Al2O3 becomes α-Al2O3. As the temperature further increases, α-Al2O3 reacts with MgO (MgO is MgO in phosphorus tailings and steel slag) to generate magnesium aluminum spinel with stable structure, wherein α-Al2O3 and MgO are both strong ionic bonds and difficult to break the bonds, so the formed magnesium aluminum spinel has high hardness and good chemical stability. Under high temperature conditions, MgO reacts with SiO2 (SiO2 is SiO2 in phosphorus tailings and steel slag), wherein MgO is a diffusion phase, diffuses to the SiO2 component in the initial stage of synthesis, and reacts to generate forsterite (melting point is 1890°C), thereby improving the refractory performance of ceramsite.

[0048] In the present invention, the main component of the fluorite tailings is SiO2, part of SiO2 reacts with CaO (CaO is CaO in phosphate tailings and steel slag) to generate wollastonite (CaSiO3), and the generated wollastonite has the characteristics of thermal stability and low water absorption; the remaining SiO2 reacts with CaO and Al2O3 (CaO and Al2O3 are CaO and Al2O3 in phosphate tailings and steel slag) to generate calcium feldspar (Ca2Al2SiO7), and calcium feldspar has the characteristics of small volume density and high strength; at the same time, under the action of iron oxide in steel slag, SiO2 in the fluorite tailings can be well transformed into phosphotquartz with a spearhead twin crystal structure, which can be embedded in the interior of ceramsite. Wollastonite, calcium feldspar and phosphotquartz with a spearhead twin crystal structure can all improve the strength of ceramsite and improve the working performance of ceramsite, so that the cylinder pressure strength of ceramsite reaches 13.5-16.1MPa.

[0049] In the present invention, (2) the dextrin is added as a binder, and its main function is: dextrin makes the raw material easier to form balls through intermolecular forces and the rheological properties of the solution. Among them, the intermolecular forces are hydrogen bonds generated between the long-chain sugar molecules during the hydrolysis process. These intermolecular forces make the solution have a certain viscosity. In addition to hydrogen bonds, the hydroxyl groups on the long-chain sugar molecules form hydrogen bonds with water molecules, further enhancing the viscosity of the solution; the rheological property of the solution is that after starch hydrolysis, the sugar molecules in the solution form a network structure with a certain fluidity. When the network structure is subjected to external force, shear stress will be generated, thereby making the solution viscous.

[0050] In the present invention, (3) the pore-forming agents activated carbon, phosphate tailings and dextrin used in the present invention effectively reduce the density of expanded clay: the sintering is an in-situ pore-forming reaction, which ensures the lightweight of expanded clay; the mechanism of the in-situ pore-forming reaction is that during the material synthesis process, cavities are formed inside the material through a specific chemical reaction or physical process, thereby completing the in-situ pore-forming reaction.

[0051] In the present invention, the specific chemical reaction or physical process includes a chemical reaction method and a thermal decomposition method, through which gas is generated, and holes are formed in the material after the gas escapes.

[0052] In the present invention, the chemical reaction method is: the activated carbon as a pore-forming agent reacts with Fe2O3 in the steel slag at high temperature to form a reaction of formulas Ⅱ to V. The generated gas is wrapped by the molten phase and can form abundant pores inside the ceramsite, thereby reducing the density of the ceramsite and promoting the lightweight development of the ceramsite.

[0053] 4Fe2O3+C→4FeO+CO2 Formula ⅠI

[0054] 2Fe2O3→4FeO+O2 Formula ⅠⅠI

[0055] C+CO2→2CO Formula ⅠV

[0056] 3C+O2→2CO+CO2 Formula V

[0057] In the present invention, the thermal decomposition method is: phosphate tailings and dextrin are decomposed at high temperature to generate gas; organic matter and dextrin in the phosphate tailings are decomposed at high temperature to generate CO2 and CO, and the generated gas forms micropores of micrometer and nanometer sizes inside the ceramsite, thereby reducing the density of the ceramsite and promoting the lightweight development of the ceramsite.

[0058] In the present invention, (4) the raw materials of the present invention contain sufficient alkaline oxides such as SiO2, Al2O3 (the sum of the contents of SiO2 and Al2O3 in siliceous phosphate tailings is more than 50%, and the SiO2 content of fluorite tailings is 70%), CaO, MgO, Na2O, K2O and Fe2O3 (the sum of the contents of CaO and MgO in steel slag is more than 50%, and siliceous phosphate tailings, washed secondary aluminum ash and fluorite tailings all include CaO, MgO, Na2O, K2O, Fe2O3 and other substances).

[0059] During the sintering process, on the one hand, since the alkaline oxide has a lower melting point, it can form a low-melting point eutectic mixture with other components, thereby reducing the overall sintering temperature. The presence of the eutectic mixture can promote the diffusion between solid phases, making the particles more tightly bound, thereby accelerating the sintering process and achieving the purpose of dissolution. On the other hand, the liquid phase formed by the alkaline metal at high temperature can serve as a diffusion medium to accelerate the diffusion between components in the raw materials, thereby eliminating pores and promoting densification, so that it can be sintered at a lower temperature. On the other hand, the presence of alkaline metals helps to form a glass phase, which can be formed at a lower temperature and can wrap and bond other solid particles, thereby promoting the densification of the sintered body.

[0060] During the sintering process, the generation of gas and glass phase occurs simultaneously. The generated gas is wrapped by the molten phase to form abundant pores inside the ceramsite, thereby reducing the density of the ceramsite and promoting the lightweight development of the ceramsite. Under the action of alkaline oxides, SiO2 and Al2O3 produce molten phases in a high temperature environment. As the sintering proceeds, the glass phase in the reaction system increases significantly and is well filled into the grains. At the same time, when the ceramsite is sintered, the heating rate of the surface of the ceramsite is higher than the heating rate inside the ceramsite, so a layer of molten phase will be generated on the surface of the ceramsite first. At this time, the generation amount and fluidity of the molten phase on the surface of the ceramsite are also higher than those inside the ceramsite. At this time, although there is foaming on the surface of the ceramsite, with the increase of the surface molten phase and the increase of fluidity, the mineral phase in the ceramsite is completely wrapped by the glass phase. At the same time, the glass phase will also cover the surface pores, thereby making the surface of the ceramsite develop towards densification. The dense surface ensures that the ceramsite has a lower apparent density and water absorption rate, which is only 3-9%. Abundant pores are formed inside the ceramsite, which reduces the density of the ceramsite. The mullite, wollastonite, anorthite, magnesia-alumina spinel and glass phase generated during the sintering process further enhance the strength of the ceramsite by encapsulating the mineral phase.

[0061] In the present invention, (5) the sintering system of ceramsite is the key to the formation of light and high-strength structure: the preheating temperature is 800-900°C, the preheating time is 10-30min, the sintering temperature is 1110-1200°C, and the sintering time is 0.5-3h. The sintering system includes a preheating stage and a sintering stage. The purpose of preheating is to remove moisture and volatile organic matter to avoid the increase in the number of cracks caused by excessive pores generated in a high-temperature environment, thereby reducing the compressive strength of the ceramsite. At the same time, it can also provide a good reducing atmosphere for sintering, so that the gas-producing substances undergo oxidation-reduction reactions to produce gas pores, forming a rich pore structure inside the ceramsite. The added pore-forming agent activated carbon can react with Fe2O3 in steel slag at high temperature to produce gas production reactions of formulas I to IV. It is necessary to set the preheating temperature to 800-900°C and the preheating time to 10-30min, because if the preheating is insufficient, it will lead to excessive gas production during the sintering process, and due to thermal shock and a large amount of gas escaping from the ceramsite, cracks will appear on the surface of the ceramsite.

[0062] In the present invention, when the sintering temperature is lower than 1110°C, less molten phase and gas are generated, which will cause the ceramsite to not expand before sintering, thereby making the strength and density of the obtained ceramsite poor; when the sintering temperature is higher than 1200°C, too much molten phase will be generated, resulting in the sintered product failing to meet the requirements for the shape of the ceramsite; when the sintering temperature is between 1110 and 1200°C, as the sintering temperature increases, the molten liquid phase gradually increases, dense enamel is generated on the surface of the ceramsite to prevent the internal gas from escaping, the water absorption rate decreases, the density increases, the excessive liquid phase fills the gas through-holes, the internal density of the ceramsite is enhanced, and the particle strength is improved.

[0063] In the present invention, when the sintering time is less than 0.5h, the sintering of the ceramsite will be incomplete; when the sintering time is longer than 3h, over-burning will occur, resulting in the problem of poor performance of the ceramsite and high energy consumption; when the sintering time is between 0.5 and 3h, as the solid phase reaction is fully carried out, within a suitable liquid phase range, the ceramsite particles are combined under the action of bonding force, and the densification degree of the ceramsite is high, thereby enhancing the strength of the ceramsite and reducing the water absorption of the ceramsite, and within the sintering time of 0.5 to 3h, the gas generated by sintering is sufficient, which promotes the expansion of the ceramsite, thereby reducing the density of the ceramsite and developing towards lightweight.

[0064] In the present invention, (6) the heat treatment (i.e., the preheating step and the sintering step) will form new phases such as glass phase and pyroxene phase, wherein the glass phase can encapsulate heavy metals, and the pyroxene phase can fix the heavy metals in the phase structure through isomorphous substitution, thereby achieving the solidification of the heavy metals. The heat treatment can also convert the heavy metals in the ceramsite from an active form of an exchangeable or reducible state to a stable form of an oxidizable or residual state, thereby further reducing the leaching concentration and the leaching toxicity, so that the obtained lightweight and high-strength ceramsite meets the safety standards, and the high heavy metal ion solidification rate (more than 95%) enables the ceramsite to be safely used in lightweight concrete.

[0065] The present invention also provides application of the lightweight high-strength ceramsite based on phosphate tailings in lightweight concrete.

[0066] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0067] In an embodiment of the present invention, the preparation method of the water-washed secondary aluminum ash is: secondary aluminum ash with a particle size of 200 μm is washed with water for 30 minutes at a mass ratio of secondary aluminum ash to water of 1:5, and then the obtained product is filtered and dried at 110° C. for 24 hours to obtain water-washed secondary aluminum ash.

[0068] Example 1

[0069] The raw materials and dosage for preparing lightweight and high-strength ceramsite are as follows:

[0070] 61 parts of siliceous phosphorus tailings (silicon dioxide content of 57wt%, particle size of 70μm), 19 parts of steel slag (the sum of calcium oxide and magnesium oxide content is 50wt%, particle size of 70μm), 10 parts of fluorite tailings (silicon dioxide content of 70wt%, particle size of 70μm), 10 parts of washed secondary aluminum ash (aluminum oxide content of 68wt%, particle size of 70μm), 3 parts of dextrin (purity of 99.9%, particle size of 5μm), 3 parts of activated carbon (purity of 99.9%, particle size of 5μm) and 5 parts of water;

[0071] Preparation of lightweight and high-strength ceramsite:

[0072] Siliceous phosphorus tailings, steel slag, fluorite tailings and washed secondary aluminum ash are mixed and ground to obtain a powder with a particle size of 200 meshes, and the obtained powder is dried at 110° C. for 24 hours to obtain a dry powder, and dextrin and activated carbon are added to the obtained dry powder to obtain a mixture;

[0073] The obtained mixture was placed in a granulator, and water was sprayed into the mixture at a rotation speed of 40 rpm to obtain spherical particles with a particle size of 12 mm. The obtained spherical particles were dried at 100° C. for 24 h to obtain dried spherical particles;

[0074] The dried spherical particles were placed in a medium temperature furnace and heated to 800°C at a heating rate of 1°C / min and kept warm for 30 minutes. The temperature was then increased to 1110°C at a heating rate of 1°C / min and kept warm for 0.5 hours before being cooled with the furnace to obtain lightweight and high-strength expanded clay.

[0075] Example 2

[0076] The raw materials and dosage for preparing lightweight and high-strength ceramsite are as follows:

[0077] 65 parts of siliceous phosphorus tailings (silicon dioxide content of 57.4wt%, particle size of 68μm), 17.5 parts of steel slag (the sum of calcium oxide and magnesium oxide content is 51wt%, particle size of 68μm), 8.5 parts of fluorite tailings (silicon dioxide content of 70.4wt%, particle size of 68μm), 9 parts of washed secondary aluminum ash (aluminum oxide content of 68.4wt%, particle size of 68μm), 3.5 parts of dextrin (purity of 99.9%, particle size of 6μm), 3.5 parts of activated carbon (purity of 99.9%, particle size of 6μm) and 6 parts of water;

[0078] Preparation of lightweight and high-strength ceramsite:

[0079] Siliceous phosphorus tailings, steel slag, fluorite tailings and washed secondary aluminum ash are mixed and ground to obtain a powder with a particle size of 200 meshes, and the obtained powder is dried at 110° C. for 24 hours to obtain a dry powder, and dextrin and activated carbon are added to the obtained dry powder to obtain a mixture;

[0080] The obtained mixture was placed in a granulator, and water was sprayed into the mixture at a rotation speed of 40 rpm to obtain spherical particles with a particle size of 10 mm. The obtained spherical particles were dried at 102.5° C. for 26 h to obtain dried spherical particles;

[0081] The dried spherical particles were placed in a medium temperature furnace and heated to 820°C at a heating rate of 1°C / min. The temperature was kept at that temperature for 25 minutes, then heated to 1130°C at a heating rate of 1°C / min. The temperature was kept at that temperature for 1.2 hours, and then cooled with the furnace to obtain lightweight and high-strength expanded clay.

[0082] Example 3

[0083] The raw materials and dosage for preparing lightweight and high-strength ceramsite are as follows:

[0084] 69 parts of siliceous phosphorus tailings (silicon dioxide content of 57.8wt%, particle size of 68μm), 16 parts of steel slag (the sum of calcium oxide and magnesium oxide content is 52wt%, particle size of 68μm), 7 parts of fluorite tailings (silicon dioxide content of 70.8wt%, particle size of 68μm), 8 parts of washed secondary aluminum ash (aluminum oxide content of 68.8wt%, particle size of 68μm), 4 parts of dextrin (purity of 99.9%, particle size of 6μm), 4 parts of activated carbon (purity of 99.9%, particle size of 6μm) and 7 parts of water;

[0085] Preparation of lightweight and high-strength ceramsite:

[0086] Siliceous phosphorus tailings, steel slag, fluorite tailings and washed secondary aluminum ash are mixed and ground to obtain a powder with a particle size of 200 meshes, and the obtained powder is dried at 110° C. for 24 hours to obtain a dry powder, and dextrin and activated carbon are added to the obtained dry powder to obtain a mixture;

[0087] The obtained mixture was placed in a granulator, and water was sprayed into the mixture at a rotation speed of 40 rpm to obtain spherical particles with a particle size of 10 mm. The obtained spherical particles were dried at 105° C. for 28 h to obtain dried spherical particles;

[0088] The dried spherical particles were placed in a medium temperature furnace and heated to 840°C at a heating rate of 2°C / min. The temperature was kept at that temperature for 20 minutes, then heated to 1150°C at a heating rate of 2°C / min. The temperature was kept at that temperature for 1.9 hours, and then cooled with the furnace to obtain lightweight and high-strength expanded clay.

[0089] Example 4

[0090] The raw materials and dosage for preparing lightweight and high-strength ceramsite are as follows:

[0091] 73 parts of siliceous phosphorus tailings (silicon dioxide content of 58.2wt%, particle size of 68μm), 14.5 parts of steel slag (the sum of calcium oxide and magnesium oxide content is 53wt%, particle size of 68μm), 5.5 parts of fluorite tailings (silicon dioxide content of 71.2wt%, particle size of 68μm), 7 parts of washed secondary aluminum ash (aluminum oxide content of 69.2wt%, particle size of 68μm), 4.5 parts of dextrin (purity of 99.9%, particle size of 6μm), 4.5 parts of activated carbon (purity of 99.9%, particle size of 6μm) and 8 parts of water;

[0092] Preparation of lightweight and high-strength ceramsite:

[0093] Siliceous phosphorus tailings, steel slag, fluorite tailings and washed secondary aluminum ash are mixed and ground to obtain a powder with a particle size of 200 meshes, and the obtained powder is dried at 110° C. for 24 hours to obtain a dry powder, and dextrin and activated carbon are added to the obtained dry powder to obtain a mixture;

[0094] The obtained mixture was placed in a granulator, and water was sprayed into the mixture at a rotation speed of 40 rpm to obtain spherical particles with a particle size of 15 mm. The obtained spherical particles were dried at 107.5° C. for 30 h to obtain dried spherical particles;

[0095] The dried spherical particles were placed in a medium temperature furnace and heated to 860°C at a heating rate of 2°C / min. The temperature was kept at that temperature for 15 minutes, then heated to 1170°C at a heating rate of 2°C / min. The temperature was kept at that temperature for 2.6 hours, and then cooled with the furnace to obtain lightweight and high-strength expanded clay.

[0096] Example 5

[0097] The raw materials and dosage for preparing lightweight and high-strength ceramsite are as follows:

[0098] 76 parts of siliceous phosphorus tailings (silicon dioxide content of 58.6wt%, particle size of 68μm), 14 parts of steel slag (the sum of calcium oxide and magnesium oxide content is 54wt%, particle size of 68μm), 5 parts of fluorite tailings (silicon dioxide content of 71.6wt%, particle size of 68μm), 5 parts of washed secondary aluminum ash (aluminum oxide content of 69.6wt%, particle size of 68μm), 5 parts of dextrin (purity of 99.9%, particle size of 6μm), 5 parts of activated carbon (purity of 99.9%, particle size of 6μm) and 9 parts of water;

[0099] Preparation of lightweight and high-strength ceramsite:

[0100] Siliceous phosphorus tailings, steel slag, fluorite tailings and washed secondary aluminum ash are mixed and ground to obtain a powder with a particle size of 200 meshes, and the obtained powder is dried at 110° C. for 24 hours to obtain a dry powder, and dextrin and activated carbon are added to the obtained dry powder to obtain a mixture;

[0101] The obtained mixture was placed in a granulator, and water was sprayed into the mixture at a rotation speed of 40 rpm to obtain spherical particles with a particle size of 10 mm. The obtained spherical particles were dried at 110° C. for 32 h to obtain dried spherical particles;

[0102] The dried spherical particles were placed in a medium temperature furnace and heated to 900°C at a heating rate of 2°C / min. The temperature was kept at that temperature for 10 minutes, then heated to 1200°C at a heating rate of 2°C / min. The temperature was kept at that temperature for 3 hours, and then cooled with the furnace to obtain lightweight and high-strength expanded clay.

[0103] The properties of the lightweight high-strength ceramsite obtained in Examples 1 to 5 were tested and Table 1 was obtained, wherein the bulk density was tested according to the national standard GB / T17431.1-2010; the cylinder pressure strength was tested according to the national standard GB / T17431.1-2010; the bulk density was tested according to the national standard GB / T17431.1-2010; the water absorption rate was tested according to the national standard GB / T17431.1-2010; the heavy metal ion solidification rate was tested according to the national standard GB5985.3-2007, and the specific test was based on the "China Solid Waste Leaching Toxicity Test Procedure-Sulfuric Acid and Nitric Acid Method" (HJ / T 299-2007), and the leaching behavior of heavy metals was analyzed.

[0104] Table 1 Performance test results of lightweight high-strength ceramsite obtained in Examples 1 to 5

[0105]

[0106]

[0107] It can be seen from Table 1 that the lightweight high-strength ceramsite prepared in Examples 1 to 5 has a volume density of 1100 to 1400 kg / m 3 The cylinder pressure strength is between 13.5 and 16.1 MPa, and the bulk density is between 550 and 670 kg / m 3 The water absorption rate is between 3% and 9%, and the solidification rate of heavy metal ions is over 95%.

[0108] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A lightweight and high-strength ceramsite based on phosphate tailings, characterized in that: It is prepared from the following raw materials in parts by weight: 61-76 parts of siliceous phosphorus tailings, 14-19 parts of steel slag, 5-10 parts of fluorite tailings, 5-10 parts of washed secondary aluminum ash, 3-5 parts of dextrin, 3-5 parts of activated carbon and 5-9 parts of water.

2. A lightweight and high-strength ceramsite based on phosphate tailings according to claim 1, characterized in that: The silicon dioxide content in the siliceous phosphorus tailings is ≥57wt%, and the particle size of the siliceous phosphorus tailings is ≤74μm.

3. A lightweight and high-strength ceramsite based on phosphate tailings according to claim 2, characterized in that: The sum of the contents of calcium oxide and magnesium oxide in the steel slag is ≥50wt%, and the particle size of the steel slag is ≤74μm.

4. A lightweight and high-strength ceramsite based on phosphate tailings according to claim 2, characterized in that: The silicon dioxide content in the fluorite tailings is ≥70wt%, and the particle size of the fluorite tailings is ≤74μm.

5. A lightweight and high-strength ceramsite based on phosphate tailings according to claim 3 or 4, characterized in that: The aluminum oxide content in the water-washed secondary aluminum ash is ≥68wt%, and the particle size of the water-washed secondary aluminum ash is ≤74μm.

6. A lightweight and high-strength ceramsite based on phosphate tailings according to claim 5, characterized in that: The purity of the dextrin is ≥99%, and the particle size of the dextrin is ≤8 μm; the purity of the activated carbon is ≥99%, and the particle size of the activated carbon is ≤8 μm.

7. A method for preparing lightweight and high-strength ceramsite based on phosphate tailings according to any one of claims 1 to 6, characterized in that: The steps include: Siliceous phosphate tailings, steel slag, fluorite tailings, washed secondary aluminum ash, dextrin, activated carbon and water are mixed and then granulated, dried, preheated and sintered in sequence to obtain lightweight and high-strength ceramsite based on phosphate tailings.

8. A method for preparing lightweight and high-strength ceramsite based on phosphate tailings according to claim 7, characterized in that: The drying temperature is 100-110° C., and the drying time is 24-32 hours.

9. A method for preparing lightweight and high-strength ceramsite based on phosphate tailings according to claim 8, characterized in that: The preheating temperature is 800-900°C, the preheating time is 10-30 minutes, the sintering temperature is 1110-1200°C, the sintering time is 0.5-3 hours, the heating rate from room temperature to the preheating temperature is 1-2°C / min, and the heating rate from the preheating temperature to the sintering temperature is 1-2°C / min.

10. Use of the lightweight high-strength ceramsite based on phosphate tailings as claimed in any one of claims 1 to 6 in lightweight concrete.

Citation Information

Patent Citations

  • Sintered ceramsite prepared by using phosphate tailings as main raw material and method

    CN106747600A

  • High-performance ceramsite based on phosphate tailings and preparation method of high-performance ceramsite

    CN114394850A

  • Lightweight high-strength ceramsite and preparation method thereof

    CN116102359A

  • Light-weight porous floor tile and manufacturing method thereof

    CN106630939A

  • Building ceramsite based on fluorite tailings and preparation method of building ceramsite

    CN113480325A

Cited By

  • Preparation method and application of modified phosphate tailing ceramsite for advanced treatment of phosphorus-containing wastewater

    CN119263874A

  • Light building ceramsite based on shield tunnel sludge, dredged sediment and phosphate tailings and preparation method thereof

    CN120004596A