Porous ceramic for electronic cigarette, preparation method and atomizing core

By using reasonable proportions of inorganic aggregate and organic solvents in the electronic cigarette ceramic atomization core, the strength and porosity of the ceramic matrix are improved, and the problems of low strength and poor atomization taste are solved, and better results are achieved The atomization and conduction effect of e-liquid improves the user experience and consistency of the product.

CN118930308APending Publication Date: 2024-11-12品度生物科技(深圳)有限公司

Patent Information

Application Number
CN202310555671.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing electronic cigarette ceramic atomization core has low strength, easy powder loss, and low atomization taste reduction degree.

Method used

Porous ceramics composed of inorganic aggregates and organic solvents are improved by reasonably proportioning inorganic adsorbents, inorganic binders, ceramic cosolvents and pore-forming agents, combined with organic reinforcement agents, to improve the strength and porosity of the ceramic matrix and reduce the sintering temperature. , avoid deformation of the thermally conductive layer and enhance the atomization effect.

Benefits of technology

It improves the strength and taste reduction of the ceramic atomized core, ensures uniform atomization and efficient conduction of e-liquid, and improves the user experience and consistency of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004232909090000081
    Figure BDA0004232909090000081
  • Figure BDA0004232909090000091
    Figure BDA0004232909090000091
  • Figure BDA0004232909090000092
    Figure BDA0004232909090000092
Patent Text Reader

Abstract

The invention relates to a porous ceramic for an electronic cigarette, a preparation method and an atomizing core, the ceramic raw material comprises an inorganic aggregate and an organic solvent, the inorganic aggregate comprises, by weight, 10-60 parts of an inorganic adsorbent, 10-40 parts of an inorganic binder, 1-30 parts of a ceramic cosolvent and 10-35 parts of a pore forming agent; the organic solvent comprises the following components in parts by weight: 10-35 parts of paraffin, 1-10 parts of beewax, 1-7 parts of an organic plasticizer and 1-5 parts of a surface modifier; wherein diatomite and attapulgite are selected as the inorganic adsorbent, one of sepiolite, vermiculite and quartz sand is added, and the organic solvent further comprises an organic enhancer and an organic binder. According to the formula of the porous ceramic for the electronic cigarette and the preparation method disclosed by the invention, the prepared porous ceramic can reach relatively high strength, powder falling of the ceramic matrix in the use process is avoided, and the atomized taste is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electronic cigarette atomization, and in particular to a porous ceramic for electronic cigarette, a preparation method and an atomization core. Background Art

[0002] The core component of electronic cigarettes is the atomizer core. Currently, the atomizer cores on the market are mainly divided into cotton core atomizer cores and ceramic atomizer cores. The advantages of cotton core atomizer cores are sufficient atomization and good taste restoration. Its disadvantages are that the pore size and porosity of the cotton core are unstable and there are large differences between batches. At the same time, the heat resistance is relatively poor, and it is easy to burn and fail at high temperatures. Due to the large pore size and porosity of the cotton core, its finished product cartridges are prone to oil leakage, affecting the product experience; the advantages of ceramic atomizer cores are good heat resistance, good taste stability in the same batch and different batches, and its finished product cartridges are not easy to leak oil, but its disadvantage is that the taste restoration is relatively poor. At the same time, the strength of the low-temperature sintered ceramic core is low, there is powder shedding of the ceramic matrix, and the thermal conductive sheet is easy to deform, which affects the oil restoration and taste.

[0003] Chinese patent CN202011570309.6 discloses an electronic cigarette atomization core made of a porous ceramic composition, which contains 0-40% purple clay, 30-70% diatomaceous earth, 1-20% quartz sand, 1-20% glass powder, and 10-50% pore-forming agent. This solves the problem that the porous ceramics in the existing technical solutions have low strength, are easily damaged and lose powder during assembly, and have poor bonding strength with metal heating circuits, which easily causes the metal heating circuit to separate from the porous ceramics and cause a burnt taste. However, for the ceramic atomization core, the problem of taste restoration has not been solved. Summary of the invention

[0004] The purpose of the present invention is to provide a porous ceramic for electronic cigarettes, a preparation method and an atomizer core, so as to solve the technical problems of the above-mentioned prior art, such as low strength, easy powder loss, and low atomization taste restoration of the electronic cigarette ceramic atomizer core.

[0005] A porous ceramic for electronic cigarettes, wherein the ceramic raw material consists of an inorganic aggregate and an organic solvent, wherein the weight ratio of the inorganic aggregate to the organic solvent is 100:30-100:40,

[0006] The inorganic aggregate comprises, by weight, 10-60 parts of an inorganic adsorbent, 10-40 parts of an inorganic binder, 1-30 parts of a ceramic cosolvent, and 10-35 parts of a pore former;

[0007] The organic solvent comprises, by weight, 10-35 parts of paraffin, 1-10 parts of beeswax, 1-7 parts of organic plasticizer, and 1-5 parts of surface modifier.

[0008] Preferably, the inorganic aggregate comprises, by weight: 30-40 parts of inorganic adsorbent, 20-30 parts of inorganic binder, 10-20 parts of ceramic solvent, and 20-30 parts of pore former; the organic solvent comprises, by weight: 20-30 parts of paraffin, 3-5 parts of beeswax, 2-6 parts of organic plasticizer, and 1-3 parts of surface modifier.

[0009] Preferably, the inorganic adsorbent comprises, by weight, 5-25 parts of diatomaceous earth, 5-10 parts of attapulgite, and 5-20 parts of sepiolite, and / or vermiculite, and / or quartz sand.

[0010] Preferably, the inorganic binder is one or more of silica sol, glass powder, silicate, phosphate, aluminate, and ethyl silicate;

[0011] The ceramic solvent is one or more of kaolin, clay, silicon powder, zinc oxide, purple clay, calcium oxide, calcium carbonate, and wollastonite;

[0012] The pore-forming agent is one or more of ultrafine PMMA powder, corn starch, pollen, pea powder, bean powder, orange peel powder, sorghum powder, barley powder, polystyrene powder, sawdust powder, carbon powder, polystyrene microspheres, linear phenolic resin composite polyethylene glycol pore-forming agent, phenolic resin pore-forming agent, and ammonium bicarbonate pore-forming agent.

[0013] Preferably, the organic solvent further comprises, by weight, 1-5 parts of an organic binder, wherein the organic binder comprises polyethylene or polypropylene.

[0014] Preferably, the organic solvent further comprises, by weight, 1-5 parts of an organic reinforcing agent, wherein the organic reinforcing agent comprises epoxy resin and polyamide.

[0015] A method for preparing porous ceramics for electronic cigarettes, comprising:

[0016] S1. Batching: weigh the materials according to the above formula with an accuracy of g to obtain an inorganic aggregate mixture and an organic solvent mixture;

[0017] S2. Mixing: Pour the inorganic aggregate mixture into the mixer, set the speed to 60r / min, and the mixing time to 2h;

[0018] S3, banburying: pour the organic solvent mixture into a banburying bin, control the temperature at 110-140°C, add the inorganic aggregate mixture stirred in step 2, set the speed to 10r / min, and banburying time to 6h;

[0019] S4, injection molding: pour the mixture after banburying in step S3 into an injection molding machine, control the temperature at 65-80°C, the pressure at 2.5-3Mpa, and hold the pressure for 20s to obtain a ceramic embryo;

[0020] S5, degreasing and sintering: placing the ceramic embryo in step S4 into a sintering furnace for degreasing and sintering, and obtaining porous ceramics after cooling.

[0021] Preferably, the degreasing sintering in step S5 is divided into seven heating stages:

[0022] Stage 1: room temperature rises to 150°C, heating time is 180 minutes, and heat preservation time is 30 minutes;

[0023] The second stage: heating from 150℃ to 200℃, heating time 50min, heat preservation time 30min;

[0024] The third stage: heating from 200℃ to 300℃, heating time 100min, heat preservation time 30min;

[0025] The fourth stage: heating from 300℃ to 350℃, heating time 50min, heat preservation time 30min;

[0026] The fifth stage: heating from 350℃ to 420℃, heating time 120min, heat preservation time 30min;

[0027] Stage 6: Heating from 420°C to 500°C, heating time 80 minutes, heat preservation time 30 minutes;

[0028] The seventh stage: heating from 500°C to 710°C, heating time 250min, heat preservation time 120min.

[0029] Furthermore, the porous ceramic for electronic cigarette obtained by the preparation method of the porous ceramic for electronic cigarette has a strength of 22-26 MPa, a thermal conductivity of 0.28-0.35 W / (m·K), a porosity of 60-64%, and a shrinkage ratio of 2.8-3.7%.

[0030] A porous ceramic atomizer core for an electronic cigarette, characterized in that it comprises the porous ceramic for an electronic cigarette according to claim 9, a heat conductive layer, a heating resistor and an electrode.

[0031] The beneficial effects of the present invention compared with the prior art include:

[0032] 1. The porous ceramic atomizer core for electronic cigarettes provided by the present invention has a ceramic raw material based on an inorganic adsorbent and an inorganic binder, which improves the strength of the ceramic matrix and prevents the ceramic matrix from falling off; at the same time, the addition of a ceramic co-solvent can reduce the sintering temperature of the ceramic, reduce the shrinkage ratio of the ceramic, and avoid deformation, warping, and shedding of the thermal conductive layer, which causes the temperature of the ceramic atomizer core to be too high during atomization and cause the core to become sticky, affecting the reduction degree and taste of the smoke oil, and even seriously exceeding the formaldehyde content, affecting the user experience of the product.

[0033] 2. The porous ceramic atomizer core for electronic cigarettes provided by the present invention can use a variety of cheap and easily available materials such as starch, pollen, bean powder, sawdust powder, etc. as pore-forming agents, which is economical and applicable. The porosity of the atomizer core reaches 60-64%, which meets the storage and conduction functions of the smoke oil during the atomization process; after testing, the thermal conductivity coefficient of the atomizer core prepared by the present invention is 0.28-0.35W / (m·K), which can better achieve the heat conduction effect during the atomization process.

[0034] 3. In order to further enhance the strength of the ceramic matrix, the present invention adds an organic reinforcing agent. During the preparation process, the epoxy resin and the polyamide undergo a ring-opening addition reaction, so that the epoxy resin is transformed from the original linear structure to a complex three-dimensional network structure, thereby further strengthening the ceramic matrix and preventing the ceramic matrix from falling off and affecting the taste experience of the ceramic atomization core during the atomization process.

[0035] 4. The porous ceramic for electronic cigarettes obtained by the preparation method provided by the present invention has a shrinkage ratio of 2.8-3.7%, and a ceramic atomizer core with small tolerance and precise size can be prepared, so that the taste consistency of the electronic cigarette is better.

[0036] 5. The porous ceramic atomizer core for electronic cigarettes provided by the present invention was installed and tested for taste, and artificial testing and evaluation were carried out from 13 dimensions, including aroma, sweetness, humidity, restoration, layering, clarity, smoke volume, coolness, satisfaction, coordination, consistency, throat hit and aftertaste, and the taste experience was better than that of existing products on the market. DETAILED DESCRIPTION

[0037] The present invention will be further described in detail below in conjunction with specific embodiments. It should be emphasized that the following description is merely exemplary and is not intended to limit the scope of the present invention and its application.

[0038] Example 1

[0039] A porous ceramic for electronic cigarettes, wherein the ceramic raw material consists of two parts: an inorganic aggregate and an organic solvent, wherein the weight ratio of the inorganic aggregate to the organic solvent is 100:40.

[0040] Specifically, the inorganic aggregate includes, by weight, 35 parts of inorganic adsorbent, 30 parts of inorganic binder, 10 parts of ceramic solvent, and 25 parts of pore former; wherein,

[0041] The inorganic adsorbent comprises, by weight, 5 parts of diatomaceous earth, 10 parts of attapulgite, 15 parts of vermiculite and 5 parts of quartz sand.

[0042] The inorganic binder comprises, by weight, 10 parts of silica sol, 10 parts of glass powder and 10 parts of ethyl silicate.

[0043] The ceramic solvent is measured by weight and includes: 10 parts of silicon micropowder.

[0044] The pore-forming agent comprises, by weight, 10 parts of ultrafine PMMA powder, 5 parts of corn starch, and 10 parts of polystyrene microspheres.

[0045] Specifically, the organic solvent includes, by weight, 28 parts of paraffin, 5 parts of beeswax, 4.6 parts of organic plasticizer, and 2.4 parts of surface modifier.

[0046] Specifically, the organic plasticizer is dibutyl phthalate.

[0047] Specifically, the surface modifier is aminopropyltrimethoxysilane.

[0048] A method for preparing porous ceramics for electronic cigarettes comprises:

[0049] S1. Batching: weigh the materials according to the above formula with an accuracy of g to obtain an inorganic aggregate mixture and an organic solvent mixture;

[0050] S2. Mixing: Pour the inorganic aggregate mixture into the mixer, set the speed to 60r / min, and the mixing time to 2h;

[0051] S3, banburying: pour the organic solvent mixture into a banburying bin, control the temperature at 110-140°C, add the inorganic aggregate mixture stirred in step 2, set the speed to 10r / min, and banburying time to 6h;

[0052] S4, injection molding: pour the mixture after banburying in step S3 into an injection molding machine, control the temperature at 65-80°C, the pressure at 2.5-3Mpa, and hold the pressure for 20s to obtain a ceramic embryo;

[0053] S5, degreasing and sintering: placing the ceramic embryo in step S4 into a sintering furnace for degreasing and sintering, and obtaining porous ceramics after cooling.

[0054] Among them, step five degreasing and sintering is divided into seven heating stages:

[0055] Stage 1: room temperature rises to 150°C, heating time is 180 minutes, and insulation time is 30 minutes;

[0056] The second stage: heating from 150℃ to 200℃, heating time 50min, holding time 30min;

[0057] The third stage: heating from 200℃ to 300℃, heating time 100min, holding time 30min;

[0058] The fourth stage: heating from 300℃ to 350℃, heating time 50min, holding time 30min;

[0059] The fifth stage: heating from 350℃ to 420℃, heating time 120min, holding time 30min;

[0060] Stage 6: 420℃ to 500℃, heating time 80min, holding time 30min;

[0061] The seventh stage: heating from 500°C to 710°C, heating time 250 minutes, holding time 120 minutes.

[0062] Example 2

[0063] A porous ceramic for electronic cigarettes, wherein the ceramic raw material consists of two parts: an inorganic aggregate and an organic solvent, wherein the weight ratio of the inorganic aggregate to the organic solvent is 100:40.

[0064] Specifically, the inorganic aggregate includes, by weight, 40 parts of inorganic adsorbent, 30 parts of inorganic binder, 10 parts of ceramic solvent, and 20 parts of pore former; wherein,

[0065] The inorganic adsorbent comprises, by weight, 10 parts of diatomaceous earth, 10 parts of attapulgite, 5 parts of vermiculite and 15 parts of quartz sand.

[0066] The inorganic binder is measured by weight and includes: 10 parts of silica sol and 20 parts of phosphate adhesive.

[0067] The ceramic solvent comprises, by weight, 5 parts of kaolin and 5 parts of wollastonite.

[0068] The pore-forming agent comprises, by weight, 5 parts of pollen, 5 parts of pea powder and 10 parts of polystyrene powder.

[0069] Specifically, the organic solvent includes, by weight, 25 parts of paraffin, 5 parts of beeswax, 3 parts of organic plasticizer, 2 parts of surface modifier, and 5 parts of organic strengthener.

[0070] Specifically, the organic plasticizer is dibutyl phthalate.

[0071] Specifically, the surface modifier is aminopropyltrimethoxysilane.

[0072] Specifically, the organic reinforcing agents are epoxy resin and polyamide. The epoxy resin and polyamide can undergo a ring-opening addition reaction, so that the epoxy resin is transformed from an original linear structure to a complex network structure, thereby strengthening the ceramic matrix and preventing the ceramic matrix from falling off.

[0073] The preparation method of the porous ceramic atomizer core for the electronic cigarette of this embodiment is the same as the preparation method of Example 1.

[0074] Example 3

[0075] A porous ceramic for electronic cigarettes, wherein the ceramic raw material consists of two parts: an inorganic aggregate and an organic solvent, wherein the weight ratio of the inorganic aggregate to the organic solvent is 100:35.

[0076] Specifically, the inorganic aggregate includes, by weight, 35 parts of inorganic adsorbent, 30 parts of inorganic binder, 15 parts of ceramic solvent, and 20 parts of pore former; wherein,

[0077] The inorganic adsorbent comprises, by weight, 15 parts of diatomaceous earth, 5 parts of attapulgite, 5 parts of sepiolite, 5 parts of vermiculite and 5 parts of quartz sand.

[0078] The inorganic binder comprises, by weight, 5 parts of silica sol, 15 parts of glass powder, 5 parts of sodium silicate and 5 parts of ethyl silicate.

[0079] The ceramic solvent comprises, by weight, 5 parts of clay, 5 parts of purple clay and 5 parts of calcium carbonate.

[0080] The pore-forming agent is measured by weight and includes: 10 parts of soybean powder and 10 parts of orange peel powder.

[0081] Specifically, the organic solvent includes, by weight, 24 parts of paraffin, 3 parts of beeswax, 6 parts of organic plasticizer, and 2 parts of surface modifier.

[0082] Specifically, the organic plasticizer is dioctyl phthalate.

[0083] Specifically, the surface modifier is aminopropyltrimethoxysilane.

[0084] The preparation method of the porous ceramic for electronic cigarette in this embodiment is the same as the preparation method in Example 1.

[0085] Example 4

[0086] A porous ceramic for electronic cigarettes, wherein the ceramic raw material consists of two parts: an inorganic aggregate and an organic solvent, wherein the weight ratio of the inorganic aggregate to the organic solvent is 100:30.

[0087] Specifically, the inorganic aggregate includes, by weight, 30 parts of inorganic adsorbent, 25 parts of inorganic binder, 20 parts of ceramic solvent, and 25 parts of pore former; wherein,

[0088] The inorganic adsorbent comprises, by weight, 20 parts of diatomaceous earth, 5 parts of attapulgite and 5 parts of quartz sand.

[0089] The inorganic binder comprises, by weight, 10 parts of phosphate adhesive, 10 parts of aluminum oxide, and 5 parts of ethyl silicate.

[0090] The ceramic flux comprises, by weight, 5 parts of silicon micropowder, 5 parts of zinc oxide, 5 parts of calcium oxide and 5 parts of wollastonite.

[0091] The pore-forming agent comprises, by weight, 10 parts of sorghum flour, 10 parts of barley flour and 5 parts of sawdust powder.

[0092] Specifically, the organic solvent includes, by weight, 20 parts of paraffin, 3 parts of beeswax, 4 parts of organic plasticizer, and 3 parts of surface modifier.

[0093] Among them, the organic plasticizer is dioctyl phthalate.

[0094] Wherein, the surface modifier is aminopropyltrimethoxysilane.

[0095] The preparation method of the porous ceramic for electronic cigarette in this embodiment is the same as the preparation method in Example 1.

[0096] Example 5

[0097] A porous ceramic for electronic cigarettes, wherein the ceramic raw material consists of two parts: an inorganic aggregate and an organic solvent, wherein the weight ratio of the inorganic aggregate to the organic solvent is 100:30.

[0098] Specifically, the inorganic aggregate includes, by weight, 35 parts of inorganic adsorbent, 20 parts of inorganic binder, 15 parts of ceramic solvent, and 30 parts of pore former; wherein,

[0099] The inorganic adsorbent comprises, by weight, 25 parts of diatomaceous earth, 5 parts of attapulgite and 5 parts of vermiculite.

[0100] The inorganic binder comprises, by weight, 5 parts of silica sol, 10 parts of glass powder and 5 parts of sodium silicate.

[0101] The ceramic solvent comprises, by weight, 5 parts of kaolin, 5 parts of clay and 5 parts of purple clay.

[0102] The pore-forming agent comprises, by weight, 10 parts of carbon powder, 5 parts of linear phenolic resin composite polyethylene glycol pore-forming agent, 10 parts of phenolic resin pore-forming agent, and 5 parts of ammonium bicarbonate pore-forming agent.

[0103] Among them, the mass percentage of linear phenolic resin in the linear phenolic resin composite polyethylene glycol pore-forming agent is 82.4%

[0104] Specifically, the organic solvent includes, by weight, 20 parts of paraffin, 4 parts of beeswax, 2 parts of organic plasticizer, 1 part of surface modifier, and 3 parts of organic binder.

[0105] Among them, the organic plasticizer is dimethyl phthalate.

[0106] Wherein, the surface modifier is aminopropyltrimethoxysilane.

[0107] Wherein, the organic binder is polyethylene.

[0108] The preparation method of the porous ceramic for electronic cigarette in this embodiment is the same as the preparation method in Example 1.

[0109] Comparative Example 1

[0110] The difference between Comparative Example 1 and Implementation 1 is that the inorganic adsorbent is 35 parts of quartz sand.

[0111] Comparative Example 2

[0112] The difference between Comparative Example 2 and Implementation 1 is that the inorganic adsorbent is 35 parts of diatomaceous earth.

[0113] Comparative Example 3

[0114] The difference between Comparative Example 3 and Implementation 1 is that the pore-forming agent is 25 parts of carbon powder.

[0115] Table 1 Ingredients of Examples 1-5 and Comparative Examples 1-3

[0116]

[0117]

[0118] The porous ceramic atomizer cores prepared in Examples 1-5 and Comparative Examples 1-3 were subjected to performance tests, and the test data were integrated, as shown in Table 2 below.

[0119] Table 2 Test properties of porous ceramics

[0120]

[0121] The porous ceramic atomizer cores prepared in Examples 1-5 and Comparative Examples 1-3 were installed to test the taste, and the test data were integrated, as shown in Table 3 below.

[0122] Table 3 Porous ceramic atomizer core installed test taste (full score 10)

[0123]

[0124] In Examples 1-5, the weight ratio of inorganic aggregate and organic solvent is reasonably controlled, a reasonable amount of inorganic binder is added to the inorganic adsorbent, and ceramic cosolvent and pore former are added, a reasonable amount of organic plasticizer and surface modifier are added to paraffin and beeswax, and an organic binder and / or organic reinforcing agent are added. Among them, the inorganic adsorbent makes the porous ceramic absorbent strong; the inorganic binder has high viscosity, which can improve the strength of the ceramic matrix and prevent the ceramic matrix from falling powder; the ceramic cosolvent is used to reduce the degreasing sintering temperature and reduce the shrinkage ratio of the porous ceramic; the pore former makes the porous ceramic have a moderate porosity; paraffin and beeswax are used as organic solvents, and the surface modifier is used to improve the compatibility of the organic solvent, so that the raw materials are easier to mix evenly; the organic plasticizer makes the ceramic embryo more plastic; the organic binder is used to improve the strength of the porous ceramic; the organic reinforcing agent plays a role in strengthening the ceramic matrix and preventing the ceramic matrix from falling powder. The porous ceramics obtained by stirring, mixing, injection molding, degreasing and sintering the above-mentioned mixture have the characteristics of high strength, moderate porosity, moderate thermal conductivity, relatively low shrinkage and high bonding rate. The ceramic atomization core prepared from the porous ceramics has the characteristics of high taste restoration.

[0125] The inorganic adsorbent in Comparative Example 1 is all quartz sand, and the other materials are the same as those in Example 1. Since quartz sand is difficult to sinter, the strength after sintering is low, and the strength decreases significantly. At the same time, due to the decrease in strength, the bonding strength between the thermal conductive layer and the ceramic substrate also decreases, resulting in a low bonding rate between the two, the thermal conductive layer warping, resulting in core sticking, poor oil reduction, and low taste evaluation.

[0126] The inorganic adsorbents in Comparative Example 2 are all diatomaceous earth, and the other materials are the same as those in Example 1. Diatomaceous earth requires a relatively high sintering temperature, but a sintering temperature that is too high will cause severe oxidation of the thermal conductive layer, increase the heating resistance, and reduce the heating efficiency; if the sintering temperature is kept at a relatively low level, the strength will drop significantly after sintering. At the same time, due to the decrease in strength, the bonding strength between the thermal conductive layer and the ceramic substrate will also decrease, resulting in a low bonding rate between the two, the thermal conductive layer will warp and cause the core to become sticky, the reduction degree of the e-liquid will deteriorate, and the taste evaluation will be low.

[0127] In Examples 1-5, the inorganic adsorbent includes at least diatomite and attapulgite, and one or more of sepiolite, vermiculite, and quartz sand are added in a reasonable manner; diatomite has a porous structure, large porosity, and strong adsorption capacity; attapulgite has a unique three-dimensional spatial chain structure and a special needle- and rod-shaped crystal structure, and has stable chemical properties, strong bonding force, and large adsorption capacity; sepiolite has the largest specific surface area among non-metallic minerals (up to 900m 2 / g) and a unique pore structure, with strong adsorption capacity; vermiculite can expand 6-20 times in volume after high temperature roasting, and has good water absorption; quartz sand has a stable structure, high temperature resistance and small expansion coefficient. Therefore, the inorganic adsorbent of the present invention adopts the above formula to make the porous ceramic have strong adsorption performance.

[0128] The pore-forming agents in Comparative Example 3 are all carbon powders, and other materials are the same as those in Example 1. The porous ceramics prepared using carbon powder as a pore-forming agent have a dense structure, good molding performance, and good taste evaluation.

[0129] The above contents are further detailed descriptions of the present invention in combination with specific / preferred implementations, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, they can also make several substitutions or modifications to these described embodiments without departing from the concept of the present invention, and these substitutions or modifications should be regarded as belonging to the protection scope of the present invention.

Claims

1. A porous ceramic for electronic cigarettes, wherein the ceramic raw material is composed of an inorganic aggregate and an organic solvent. It is characterized in that The weight ratio of the inorganic aggregate to the organic solvent is 100:30-100:40, The inorganic aggregate comprises, by weight, 10-60 parts of an inorganic adsorbent, 10-40 parts of an inorganic binder, 1-30 parts of a ceramic cosolvent, and 10-35 parts of a pore former; The organic solvent comprises, by weight, 10-35 parts of paraffin, 1-10 parts of beeswax, 1-7 parts of organic plasticizer, and 1-5 parts of surface modifier.

2. The porous ceramic for electronic cigarette according to claim 1, It is characterized in that The inorganic aggregate comprises, by weight, 30-40 parts of inorganic adsorbent, 20-30 parts of inorganic binder, 10-20 parts of ceramic solvent aid, and 20-30 parts of pore former; the organic solvent comprises, by weight, 20-30 parts of paraffin, 3-5 parts of beeswax, 2-6 parts of organic plasticizer, and 1-3 parts of surface modifier.

3. The porous ceramic for electronic cigarette according to claim 2, It is characterized in that The inorganic adsorbent comprises, by weight, 5-25 parts of diatomaceous earth, 5-10 parts of attapulgite, and 5-20 parts of sepiolite, and / or vermiculite, and / or quartz sand.

4. The porous ceramic for electronic cigarette according to claim 2, It is characterized in that The inorganic binder is one or more of silica sol, glass powder, silicate, phosphate, aluminate, and ethyl silicate; And / or, the ceramic solvent is one or more of kaolin, clay, silicon powder, zinc oxide, purple clay, calcium oxide, calcium carbonate, and wollastonite; And / or, the pore-forming agent is one or more of ultrafine PMMA powder, corn starch, pollen, pea powder, bean powder, orange peel powder, sorghum powder, barley powder, polystyrene powder, sawdust powder, carbon powder, polystyrene microspheres, linear phenolic resin composite polyethylene glycol pore-forming agent, phenolic resin pore-forming agent, and ammonium bicarbonate pore-forming agent.

5. The porous ceramic for electronic cigarette according to claim 1, It is characterized in that The organic solvent further comprises, by weight, 1-5 parts of an organic binder, wherein the organic binder comprises polyethylene or polypropylene.

6. The porous ceramic for electronic cigarette according to claim 1, It is characterized in that The organic solvent further comprises, by weight, 1-5 parts of an organic reinforcing agent, wherein the organic reinforcing agent comprises epoxy resin and polyamide.

7. A method for preparing porous ceramics for electronic cigarettes, include: S1. Batching: weighing materials according to the formula described in any one of claims 1 to 6 with an accuracy of g to obtain an inorganic aggregate mixture and an organic solvent mixture; S2. Mixing: Pour the inorganic aggregate mixture into the mixer, set the speed to 60r / min, and the mixing time to 2h; S3, banburying: pour the organic solvent mixture into a banburying bin, control the temperature at 110-140°C, add the inorganic aggregate mixture stirred in step 2, set the speed to 10r / min, and banburying time to 6h; S4, injection molding: pour the mixture after banburying in step S3 into an injection molding machine, control the temperature at 65-80°C, the pressure at 2.5-3Mpa, and hold the pressure for 20s to obtain a ceramic embryo; S5, degreasing and sintering: placing the ceramic embryo in step S4 into a sintering furnace for degreasing and sintering, and obtaining porous ceramics after cooling.

8. The method for preparing the porous ceramic for electronic cigarette according to claim 7, It is characterized in that The debinding sintering in step S5 is divided into seven heating stages: Stage 1: room temperature rises to 150°C, heating time is 180 minutes, and heat preservation time is 30 minutes; The second stage: heating from 150℃ to 200℃, heating time 50min, heat preservation time 30min; The third stage: heating from 200℃ to 300℃, heating time 100min, heat preservation time 30min; The fourth stage: heating from 300℃ to 350℃, heating time 50min, heat preservation time 30min; The fifth stage: heating from 350℃ to 420℃, heating time 120min, heat preservation time 30min; Stage 6: Heating from 420°C to 500°C, heating time 80 minutes, heat preservation time 30 minutes; The seventh stage: heating from 500°C to 710°C, heating time 250min, heat preservation time 120min.

9. The porous ceramic for electronic cigarette obtained by the preparation method according to claim 8, It is characterized in that The porous ceramic for electronic cigarette has a strength of 22-26 MPa, a thermal conductivity of 0.28-0.35 W / (m·K), a porosity of 60-64%, and a shrinkage ratio of 2.8-3.7%.

10. A porous ceramic atomizer core for electronic cigarettes, It is characterized in that It comprises the porous ceramic for electronic cigarette according to claim 9, a heat conductive layer, a heating resistor and an electrode.

Citation Information

Patent Citations

  • Ceramic core surface room temperature hardening agent and ceramic core surface hardening process

    CN102432338A

  • Porous ceramic for electronic cigarette and preparation method thereof

    CN111205104A

  • Porous ceramic composition and preparation method thereof and electronic cigarette atomization core using ceramic composition

    CN112679202A

  • Porous ceramic material and preparation method thereof, heating assembly, atomizer and electronic cigarette

    CN114149248A

  • Large-aperture high-strength ceramic atomizing core and preparation method thereof

    CN116098320A

Cited By

  • Purple sand sintered body for cigarette aroma enhancement as well as preparation method and application of purple sand sintered body

    CN120554085A