Multistage porous ceramic, preparation method thereof and atomizing core

Through the preparation method of multi-stage porous ceramics, drying foaming and degreasing sintering treatments, porous ceramics with large internal pore sizes and small surface pore sizes are formed, which solves the problem of insufficient liquid conduction rate and liquid storage properties, and achieves efficient liquid conduction and Locking effect.

CN118930309APending Publication Date: 2024-11-12SHENZHEN JIJIA NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411013813.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing porous ceramic preparation methods cannot take into account both the liquid conduction rate and the liquid locking property, and the internal pore size is small, resulting in insufficient liquid conduction rate and liquid storage property.

Method used

By adopting the preparation method of multi-stage porous ceramics, the mixing, stirring, molding, drying and foaming, and degreasing sintering of the frame powder, pore-forming agent, adhesive and solvent, the pore diameter is formed, while maintaining the surface pore diameter. Smaller, ensuring liquid conductivity and liquid storage.

Benefits of technology

The liquid conductivity and liquid storage properties of porous ceramics have been improved, with large internal pore size, high porosity, small surface pore size, and good liquid locking properties, which solves the problem of insufficient liquid conductivity and liquid storage properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930309A_ABST
    Figure CN118930309A_ABST
Patent Text Reader

Abstract

The embodiment of the invention belongs to the technical field of atomizing cores, and relates to multistage porous ceramic, a preparation method thereof and an atomizing core, and the preparation method of the multistage porous ceramic comprises the following steps: providing skeleton powder, a pore forming agent, an adhesive and a solvent; mixing the skeleton powder, a pore forming agent, an adhesive and a solvent to form a first mixture; stirring the first mixture to form a second mixture; modeling the second mixture to form a third mixture; drying and foaming the third mixture to obtain a fourth mixture; and degreasing and sintering the fourth mixture to obtain the multistage porous ceramic. The pore-forming agent and the adhesive in the third mixture are subjected to a foaming reaction through drying and foaming treatment, and a large internal pore diameter is formed. As the internal and external pressure difference and surface solvent evaporation of the third mixture are fast in the drying and foaming process, the surface aperture is small. In conclusion, the multistage porous ceramic is large in internal pore diameter, good in liquid guiding performance, high in porosity, good in liquid storage performance, small in surface pore diameter and good in liquid locking performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of atomizer cores, and more specifically, to a multi-stage porous ceramic and a preparation method thereof, and an atomizer core. Background Art

[0002] Existing aerosol generating devices usually include an atomizer core, which can heat the liquid to be heated so that the liquid to be heated forms an aerosol, and then the aerosol flows to the external environment through the airway for the user to inhale. The material of the atomizer core is usually porous ceramic.

[0003] The size of the internal pore size of porous ceramics directly affects the liquid conduction rate. Generally, the larger the pore size, the higher the liquid conduction rate. However, if the internal pore size of the porous ceramic is too large, it is easy to cause internal liquid leakage. Therefore, the porous ceramics prepared by the preparation method of porous ceramics in the prior art cannot take into account the liquid conduction rate, liquid locking and liquid storage at the same time, and the internal pore size is small. Summary of the invention

[0004] The technical problem to be solved by the embodiments of the present application is that the porous ceramics prepared by the existing porous ceramic preparation method cannot take into account both the liquid conduction rate and the liquid lock, and the internal pore size is relatively small.

[0005] In order to solve the above technical problems, the embodiment of the present application adopts the following solution:

[0006] A method for preparing a multi-level porous ceramic, the method comprising:

[0007] Provide skeleton powder, pore-forming agent, adhesive and solvent;

[0008] Mixing the skeleton powder, the pore-forming agent, the adhesive and the solvent to form a first mixture;

[0009] Stirring the first mixture to form a second mixture;

[0010] performing shaping treatment on the second mixture to form a third mixture;

[0011] performing a drying and foaming process on the third mixture to obtain a fourth mixture;

[0012] The fourth mixture is subjected to degreasing and sintering treatment to obtain multi-level porous ceramics.

[0013] Furthermore, the modeling process comprises:

[0014] providing a basement membrane;

[0015] Applying the second mixture on the surface of the base film to form a slurry film layer;

[0016] The slurry film layer is allowed to stand to obtain a third mixture;

[0017] Wherein, the thickness of the slurry film layer is 3 mm to 5 mm; and / or,

[0018] The standing treatment time is 30 min to 60 min.

[0019] Furthermore, the temperature of the drying treatment is 50° C. to 80° C.; and / or the time of the drying treatment is 1 hour to 5 hours.

[0020] Further, the temperature of the degreasing sintering furnace is increased from 25° C. to a first temperature;

[0021] Under a first temperature condition, performing a first heat preservation treatment for a first time period;

[0022] Raising the temperature of the degreasing sintering furnace from a first temperature to a second temperature;

[0023] Under the second temperature condition, performing a second heat preservation treatment for a second time period;

[0024] Raising the temperature of the degreasing sintering furnace from the second temperature to a third temperature;

[0025] Under the third temperature condition, performing a third heat preservation treatment for a third time period;

[0026] raising the temperature of the degreasing sintering furnace from the third temperature to the fourth temperature;

[0027] Under a fourth temperature condition, performing a fourth heat preservation treatment for a fourth period of time;

[0028] Wherein, the first temperature is 25°C to 300°C; and / or,

[0029] The first duration is 30 minutes to 60 minutes; and / or,

[0030] The second temperature is 300° C. to 500° C., and / or

[0031] The second duration is 30 minutes to 60 minutes; and / or,

[0032] The third temperature is 500° C. to 750° C.; and / or,

[0033] The third duration is 30 minutes to 60 minutes; and / or,

[0034] The fourth temperature is 750°C to 1280°C; and / or,

[0035] The fourth duration is 100 minutes to 180 minutes; and / or,

[0036] In the step of increasing the temperature from 25°C to the first temperature, the heating rate is 2°C / min to 3°C / min; and / or,

[0037] In the step of increasing the temperature from the first temperature to the second temperature, the heating rate is 3°C / min to 5°C / min; and / or,

[0038] In the step of increasing the temperature from the second temperature to the third temperature, the heating rate is 5°C / min to 10°C / min; and / or,

[0039] In the step of increasing the temperature from the third temperature to the fourth temperature, the heating rate is 10° C. / min to 15° C. / min.

[0040] Further, the skeleton powder includes at least one of quartz powder, aluminum silicate, and talc; and / or,

[0041] The pore-forming agent comprises at least one of polystyrene microspheres and methyl methacrylate; and / or,

[0042] The adhesive comprises at least one of carboxymethyl cellulose and ethyl cellulose; and / or,

[0043] The solvent includes at least one of pinol and ethanol.

[0044] Furthermore, the skeleton powder is selected from quartz powder, aluminum silicate, calcium carbonate, and talc, the pore-forming agent is polystyrene microspheres, the adhesive is ethyl cellulose, and the solvent is ethanol and pinol.

[0045] The weight ratio of the quartz powder to the first mixture is 25% to 30%, the weight ratio of the aluminum silicate to the first mixture is 5% to 10%, the weight ratio of the calcium carbonate to the first mixture is 1% to 2.5%, the weight ratio of the talc to the first mixture is 3% to 5%, the weight ratio of the polystyrene microspheres to the first mixture is 20% to 25%, the weight ratio of the ethyl cellulose to the first mixture is 2% to 3%, the weight ratio of the pinol alcohol to the first mixture is 12% to 18%, and the weight ratio of the ethanol to the first mixture is 20% to 25%.

[0046] Furthermore, the step of mixing the skeleton powder, the pore-forming agent, the adhesive and the solvent to form a first mixture comprises:

[0047] Adding the skeleton powder, the pore-forming agent, the adhesive and the solvent into a stirring device;

[0048] immersing a stirring device in water, starting the stirring device, and sealing and stirring to form a first mixture;

[0049] Wherein, the temperature of the water is 55°C to 65°C; and / or,

[0050] The sealing stirring time is 3h to 6h.

[0051] Correspondingly, the present application also provides a multi-level porous ceramic, which is prepared by the preparation method of the multi-level porous ceramic described in any one of the above embodiments.

[0052] Furthermore, the multi-level porous ceramic is provided with internal through holes and surface through holes, the surface through holes connect the internal through holes with the external environment, the pore size of the surface through holes is 15 microns to 35 microns, and the pore size of the internal through holes is 100 microns to 1000 microns.

[0053] Correspondingly, the present application also provides an atomizer core, the components of the atomizer core include the multi-level porous ceramic described in any one of the above embodiments; or, the components of the atomizer core include the multi-level porous ceramic prepared by the preparation method of the multi-level porous ceramic described in any one of the above embodiments.

[0054] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0055] Because the third mixture has been dried and foamed, the pore-forming agent and adhesive inside it will produce a foaming reaction, thereby expanding the space inside the third mixture, thereby forming a larger internal pore size and a higher porosity. At the same time, due to the internal and external pressure difference and the rapid evaporation of the surface solvent in the drying and foaming process of the third mixture, the surface pore size of the multi-level porous ceramic is relatively small. In summary, the multi-level porous ceramic has a large internal pore size, good liquid conductivity, high porosity, good liquid storage, a small surface pore size, and good liquid locking properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] In order to more clearly illustrate the solutions in the present application or the prior art, a brief introduction is given below to the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0057] Figure 1 is a flow chart of a method for preparing multi-level porous ceramics according to an embodiment of the present application;

[0058] Figure 2 It is a schematic diagram of the surface condition of the multi-level porous ceramic sample in the test of Example 1 of the present application. DETAILED DESCRIPTION

[0059] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0060] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.

[0061] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0062] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0063] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0064] Please refer to Figure 1The present application provides a method for preparing a multi-level porous ceramic, the method comprising:

[0065] S100, provides skeleton powder, pore-forming agent, adhesive and solvent;

[0066] S200, mixing the skeleton powder, the pore-forming agent, the adhesive and the solvent to form a first mixture;

[0067] S300, stirring the first mixture to form a second mixture;

[0068] S400, performing shaping processing on the second mixture to form a third mixture;

[0069] S500, performing a drying and foaming process on the third mixture to obtain a fourth mixture;

[0070] S600, performing degreasing and sintering treatment on the fourth mixture to obtain a multi-level porous ceramic.

[0071] In this embodiment, the solvent can wet the skeleton powder, pore former and adhesive, so that the first mixture after mixing is a slurry structure, which is convenient for uniform stirring. The stirring process can make the pore former in the second mixture evenly distributed, so that the pore size distribution inside the multi-level porous ceramic formed subsequently is uniform. The molding process can give the second mixture a certain shape, which is convenient for subsequent drying and foaming treatment and subsequent production and processing. For example, if the multi-level porous ceramic produced subsequently is a sheet structure, the third mixture can be molded into a sheet structure during the molding process.

[0072] Drying and foaming the third mixture can cause the pore-forming agent and adhesive in the third mixture to undergo a foaming reaction, because during the drying process, first, the solvent evaporation rate on the surface of the third mixture is faster, while the solvent evaporation rate inside is relatively slow. Secondly, during the drying and foaming process, the solvent and gas inside the third mixture are subject to different external and internal pressures, resulting in differences in pore size, and this difference leads to different pore structures on the surface and inside. As a result, the fourth mixture finally formed has large pores inside, while the surface hardly changes. Degreasing and sintering can remove residual solvents, low-temperature volatile substances, and adhesives in the fourth mixture and allow the fourth mixture to form a solid.

[0073] In summary, the multi-level porous ceramic of this embodiment has a small surface pore size, so it can lock liquid, and has a large internal pore size, so its liquid conductivity is high, and because of its high porosity, it has good liquid storage performance.

[0074] Further, the steps of modeling processing include:

[0075] providing a basement membrane;

[0076] Applying the second mixture on the surface of the base film to form a slurry film layer;

[0077] The slurry film layer is allowed to stand to obtain a third mixture;

[0078] Wherein, the thickness of the slurry film layer is 3 mm to 5 mm; and / or,

[0079] The static treatment time is 30min to 60min.

[0080] In this embodiment, by coating the second mixture on the surface of the base film to form a slurry film layer, the shape of the multi-level porous ceramic can be determined to form a sheet structure. The multi-level porous ceramic with a sheet structure has wide applicability, is easy to process, and can effectively reduce production costs.

[0081] Furthermore, the drying temperature is 50°C to 80°C;

[0082] And / or, the drying time is 1 hour to 5 hours.

[0083] In this embodiment, the temperature and time of the drying process will affect the porosity and internal pore size of the multi-level porous ceramics finally formed. If the temperature is too high or the time is too long, the following problems may occur: excessive reaction of the pore former and the adhesive, resulting in the multi-level porous ceramics having too large internal pores; premature decomposition of the internal pore former and other structures to form an effective pore structure; surface hardening to form a dense layer affects the evaporation of the internal solvent, thereby increasing the internal pressure of the multi-level porous ceramics and forming cracks or defects; rapid evaporation of the surface liquid causes the surface pores to be too small.

[0084] Therefore, the temperature and time of the drying process in this embodiment can ensure that the multi-level porous ceramics finally formed have a smaller surface pore size, a larger internal pore size, and higher strength.

[0085] Further, the temperature of the degreasing sintering furnace is increased from 25° C. to a first temperature;

[0086] Under a first temperature condition, performing a first heat preservation treatment for a first time period;

[0087] Raising the temperature of the degreasing sintering furnace from a first temperature to a second temperature;

[0088] Under the second temperature condition, performing a second heat preservation treatment for a second time period;

[0089] Raising the temperature of the degreasing sintering furnace from the second temperature to a third temperature;

[0090] Under the third temperature condition, performing a third heat preservation treatment for a third time period;

[0091] raising the temperature of the degreasing sintering furnace from the third temperature to the fourth temperature;

[0092] Under a fourth temperature condition, performing a fourth heat preservation treatment for a fourth period of time;

[0093] Wherein, the first temperature is 25°C to 300°C; and / or,

[0094] The first duration is 30 minutes to 60 minutes; and / or,

[0095] The second temperature is 300° C. to 500° C., and / or

[0096] The second duration is 30 minutes to 60 minutes; and / or,

[0097] The third temperature is 500° C. to 750° C.; and / or,

[0098] The third duration is 30 minutes to 60 minutes; and / or,

[0099] The fourth temperature is 750°C to 1280°C; and / or,

[0100] The fourth duration is 100 minutes to 180 minutes; and / or,

[0101] In the step of increasing the temperature from 25°C to the first temperature, the heating rate is 2°C / min to 3°C / min; and / or,

[0102] In the step of increasing the temperature from the first temperature to the second temperature, the heating rate is 3°C / min to 5°C / min; and / or,

[0103] In the step of increasing the temperature from the second temperature to the third temperature, the heating rate is 5°C / min to 10°C / min; and / or,

[0104] In the step of increasing the temperature from the third temperature to the fourth temperature, the heating rate is 10° C. / min to 15° C. / min.

[0105] In this embodiment, the first heat preservation treatment of degreasing and sintering can remove the residual solvent and low-temperature volatile substances in the fourth mixture, the second heat preservation treatment can remove the adhesive, partially decompose and carbonize it at high temperature, and the third heat preservation treatment can remove the residual carbonized material, so that the fourth mixture can be debonded and form a porous structure. The first three heat preservations are degreasing steps, and the last fourth heat preservation is a sintering step, which can shape the fourth mixture and retain the porous structure. After the fourth heat preservation, the heating can be stopped and the furnace can be cooled to obtain a multi-level porous ceramic.

[0106] Further, the skeleton powder includes at least one of quartz powder, aluminum silicate, and talc; and / or,

[0107] The pore-forming agent includes at least one of polystyrene microspheres and methyl methacrylate; and / or,

[0108] The adhesive comprises at least one of carboxymethyl cellulose and ethyl cellulose; and / or,

[0109] The solvent includes at least one of pinol and ethanol.

[0110] In this embodiment, the combination of skeleton powder, pore former, adhesive and solvent can ensure that the first mixture is in a slurry state, and can also form relatively large internal pores in the subsequent drying and foaming process.

[0111] Furthermore, the skeleton powder is selected from quartz powder, aluminum silicate, calcium carbonate, and talc, the pore-forming agent is polystyrene microspheres, the adhesive is ethyl cellulose, and the solvent is ethanol and pinol.

[0112] The weight ratio of quartz powder to the first mixture is 25% to 30%, the weight ratio of aluminum silicate to the first mixture is 5% to 10%, the weight ratio of calcium carbonate to the first mixture is 1% to 2.5%, the weight ratio of talc to the first mixture is 3% to 5%, the weight ratio of polystyrene microspheres to the first mixture is 20% to 25%, the weight ratio of ethyl cellulose to the first mixture is 2% to 3%, the weight ratio of pinol to the first mixture is 12% to 18%, and the weight ratio of ethanol to the first mixture is 20% to 25%.

[0113] In this embodiment, the ratio of the pore former and the adhesive can make the number of internal pores of the finally prepared multi-level porous ceramic moderate and ensure a certain strength of the multi-level porous ceramic. The proportion of the solvent can ensure that the first mixture is in a slurry state and the components inside the first mixture are fully wetted. The ratio of each material of the skeleton powder can change the porosity and structural strength of the multi-level porous ceramic.

[0114] Furthermore, the step of mixing the skeleton powder, the pore-forming agent, the adhesive and the solvent to form a first mixture comprises:

[0115] Adding skeleton powder, pore former, adhesive and solvent into a stirring device;

[0116] immersing a stirring device in water, starting the stirring device, and sealing and stirring to form a first mixture;

[0117] Wherein, the temperature of water is 55°C to 65°C; and / or,

[0118] The sealed stirring time is 3h to 6h.

[0119] In this embodiment, first, the material is placed in a water bath and heated to 55°C to 65°C to increase the temperature and thereby reduce the viscosity of the slurry; secondly, it is stirred in a sealed environment for 3 to 6 hours to ensure that the components are fully mixed to form a uniform ceramic slurry; then, through the combined effects of temperature and stirring, precipitation or stratification of heavy components is prevented, the fluidity of the slurry is improved, and better operability is provided for subsequent coating and molding.

[0120] Correspondingly, the present application also provides a multi-level porous ceramic, which is prepared by the preparation method of the multi-level porous ceramic in any one of the above embodiments.

[0121] In this embodiment, since the multi-level porous ceramic is prepared by the preparation method of the multi-level porous ceramic in any of the above embodiments, the internal pore size of the multi-level porous ceramic is larger, the surface pore size is smaller, and the internal pore size is larger than that of the prior art, so it has good liquid conductivity, porosity and liquid locking.

[0122] Furthermore, the multi-level porous ceramic is provided with internal through holes and surface through holes, the surface through holes connect the internal through holes with the external environment, the pore size of the surface through holes is 15 microns to 35 microns, and the pore size of the internal through holes is 100 microns to 1000 microns.

[0123] In this embodiment, since the aperture of the surface through-holes of the multi-level porous ceramic is 15 microns to 35 microns, it can effectively lock the liquid and prevent the liquid from flowing out from the internal through-holes. The aperture range of the internal through-holes can ensure that the liquid conductivity and porosity of the multi-level porous ceramic are high.

[0124] Correspondingly, the present application also provides an atomizer core, the components of the atomizer core include the multi-level porous ceramic of any one of the above embodiments; or, the components of the atomizer core include the multi-level porous ceramic prepared by the preparation method of the multi-level porous ceramic of any one of the above embodiments.

[0125] In this embodiment, the components of the atomizer core include the multi-level porous ceramics of any one of the above embodiments; or, the components of the atomizer core include the multi-level porous ceramics prepared by the preparation method of the multi-level porous ceramics of any one of the above embodiments. Therefore, the atomizer core has a higher liquid conductivity and can effectively prevent liquid from leaking from the inside.

[0126] Next, the performance of the multi-level porous ceramic in this scheme is further analyzed through examples, as shown in the following examples:

[0127] Example 1

[0128] The preparation method of the multi-stage porous ceramic atomization core material of this embodiment is as follows:

[0129] Step 1, prepare the first mixture. Provide 28wt% quartz powder, 6wt% aluminum silicate, 2wt% calcium carbonate, 4wt% talc, 22wt% polystyrene microspheres, 2wt% ethyl cellulose powder, 14wt% pinoline, and 22wt% ethanol. Quartz powder, aluminum silicate, calcium carbonate, and talc are skeleton powders; polystyrene microspheres are pore-forming agents; ethyl cellulose is an adhesive; and pinoline and ethanol are solvents.

[0130] Weigh the above materials according to the above proportions into a stirring bucket to form a first mixture. Place the stirring bucket in a water bath at 60°C, seal and stir for 4 hours to form a uniform second mixture.

[0131] Step 2: coating and molding. The second mixture obtained in step 1 is applied to the flat surface of the PET release film with a coater to form a third mixture. The coating thickness of the third mixture is 4 mm. The third mixture is allowed to stand for 55 minutes to allow the third mixture to be leveled and evenly formed.

[0132] Step 3, drying and foaming, the third mixture obtained in step 2 is placed in a blast drying oven for drying at a temperature of 65°C for 2 hours. During the drying process, the residual solvent in the third mixture reacts with the pore-forming agent and the adhesive to form a foaming reaction, and a super-large pore size is formed inside the third mixture, while the surface does not change. Thus, a fourth mixture is formed.

[0133] Step 4, degreasing and high-temperature sintering the fourth mixture obtained in step 3, adopting degreasing and sintering integrated molding, the degreasing process conditions are: ① room temperature-300°C, heating rate 2°C / min; ② 300°C-300°C, insulation for 30min, removing the residual solvent and low-temperature volatile substances in the fourth mixture; ③ 300-500°C, heating rate 3°C / min; ④ 500°C-500°C, insulation for 30min, removing the adhesive, decomposing and removing it at high temperature and carbonizing it; ⑤ 500-750℃, heating rate 5℃ / min; ⑥750℃-750℃, keep warm for 60min, remove residual carbon, make the fourth mixture completely debind before sintering, and form a porous structure; sintering process conditions ⑦750℃-1280℃, heating rate 10℃ / min; ⑧1280℃-1280℃, keep warm for 120min, sinter the fourth mixture and retain the porous structure, then stop heating and cool down with the furnace to obtain multi-level porous ceramics.

[0134] Example 2

[0135] This embodiment is basically the same as Embodiment 1, except that the coating thickness of the third mixture used in step 2 of the present application is 3 mm.

[0136] Example 3

[0137] This embodiment is basically the same as Embodiment 1, except that the coating thickness of the third mixture used in step 2 of the present application is 5 mm.

[0138] Example 4

[0139] This embodiment is basically the same as Embodiment 1, except that the drying temperature in step 3 of the present application is 50°C.

[0140] Example 5

[0141] This embodiment is basically the same as Embodiment 1, except that the drying temperature in step 3 of the present application is 80°C.

[0142] Example 6

[0143] This embodiment is basically the same as Embodiment 1, except that in step 1 of the present application, the weight ratio of quartz powder is adjusted to 30%, and the weight ratio of polystyrene microspheres is adjusted to 20%.

[0144] Example 7

[0145] This embodiment is basically the same as Embodiment 1, except that in step 1 of the present application, the weight ratio of quartz powder is adjusted to 25%, and the weight ratio of polystyrene microspheres is adjusted to 25%.

[0146] Comparative Example

[0147] The steps of this comparative example are basically the same as those of Example 1, except that step two and step three are replaced by: putting the kneaded second mixture into an extruder for extrusion molding to prepare the required porous third mixture, and then putting the third mixture into a drying furnace at 60°C for drying for 2 hours.

[0148] Under the same conditions, the porosity of Examples 1 to 7 and the comparative example was tested using a porosity tester, and the time taken by the porous multi-level ceramic to absorb liquid from blank was measured by a stopwatch.

[0149] According to observation and measurement, the above examples 1 to 3 and the comparative example are compared to form Table 1:

[0150] Test items Porosity (%) Absorption time (S) Example 1 69.85 5.5 Example 2 62.34 6.2 Example 3 74.52 5.8 Example 4 58.45 6.9 Example 5 78.23 5.1 Example 6 68.89 5.4 Example 7 69.11 5.5 Comparative Example 50.51 8.5

[0151] Table 1

[0152] According to the above table:

[0153] According to the data of Example 1 and the comparative example, compared with the traditional extrusion molding process, the internal pore size of the multi-level porous ceramic finally formed in Example 1 through the drying and foaming process is larger, so its liquid absorption time is shorter, and the porosity is higher, so its liquid storage performance is higher. Therefore, compared with the prior art, the multi-level porous ceramic prepared in the embodiment of the present application has a high porosity and a large internal pore size, and can be observed by the naked eye (such as Figure 2 It can be seen that the pore size on its surface is relatively small.

[0154] According to Example 1 and Examples 2-3, the porosity of Example 2 is less than that of Example 1, and the liquid conduction time is longer than that of Example 1, while the porosity of Example 3 is greater than that of Example 1, and the liquid conduction time is shorter than that of Example 1. Therefore, the thickness of the coating molding can affect the porosity and internal pore size of the finally formed multi-level porous ceramic.

[0155] According to Example 1 and Examples 4 to 5, it can be seen that the porosity and the internal pore size increase as the drying temperature increases, and the porosity and the internal pore size decrease as the drying temperature decreases.

[0156] According to Example 1 and Examples 6 to 7, adjusting the proportion of each component of the skeleton powder of the multi-level porous ceramic can affect the porosity and internal pore size of the multi-level porous ceramic to a certain extent, but the scope of the influence is relatively small.

[0157] Obviously, the embodiments described above are only some embodiments of the present application, rather than all embodiments. The preferred embodiments of the present application are given in the accompanying drawings, but they do not limit the patent scope of the present application. The present application can be implemented in many different forms. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive. Although the present application is described in detail with reference to the aforementioned embodiments, for those skilled in the art, it is still possible to modify the technical solutions recorded in the aforementioned specific implementation methods, or to perform equivalent replacement of some of the technical features therein. Any equivalent structure made using the contents of the specification and drawings of this application, directly or indirectly used in other related technical fields, is similarly within the scope of patent protection of this application.

[0158] Although the embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, combinations, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present invention is defined by the claims and their equivalents.

Claims

1. A method for preparing a multi-level porous ceramic, characterized in that: The method comprises: Provide skeleton powder, pore-forming agent, adhesive and solvent; Mixing the skeleton powder, the pore-forming agent, the adhesive and the solvent to form a first mixture; Stirring the first mixture to form a second mixture; performing shaping treatment on the second mixture to form a third mixture; performing a drying and foaming process on the third mixture to obtain a fourth mixture; The fourth mixture is subjected to degreasing and sintering treatment to obtain multi-level porous ceramics.

2. The method for preparing the multi-level porous ceramic according to claim 1, characterized in that: The steps of the modeling process include: providing a basement membrane; Applying the second mixture on the surface of the base film to form a slurry film layer; The slurry film layer is allowed to stand to obtain a third mixture; Wherein, the thickness of the slurry film layer is 3 mm to 5 mm; and / or, The standing treatment time is 30 min to 60 min.

3. The method for preparing the multi-level porous ceramic according to claim 1, characterized in that: The drying treatment temperature is 50° C. to 80° C.; and / or the drying treatment time is 1 hour to 5 hours.

4. The method for preparing the multi-level porous ceramic according to claim 1, characterized in that: Raising the temperature of the degreasing sintering furnace from 25° C. to a first temperature; Under a first temperature condition, performing a first heat preservation treatment for a first time period; Raising the temperature of the degreasing sintering furnace from a first temperature to a second temperature; Under the second temperature condition, performing a second heat preservation treatment for a second time period; Raising the temperature of the degreasing sintering furnace from the second temperature to a third temperature; Under the third temperature condition, performing a third heat preservation treatment for a third time period; raising the temperature of the degreasing sintering furnace from the third temperature to the fourth temperature; Under a fourth temperature condition, performing a fourth heat preservation treatment for a fourth period of time; Wherein, the first temperature is 25°C to 300°C; and / or, The first duration is 30 minutes to 60 minutes; and / or, The second temperature is 300° C. to 500° C., and / or The second duration is 30 minutes to 60 minutes; and / or, The third temperature is 500° C. to 750° C.; and / or, The third duration is 30 minutes to 60 minutes; and / or, The fourth temperature is 750°C to 1280°C; and / or, The fourth duration is 100 minutes to 180 minutes; and / or, In the step of increasing the temperature from 25°C to the first temperature, the heating rate is 2°C / min to 3°C / min; and / or, In the step of increasing the temperature from the first temperature to the second temperature, the heating rate is 3°C / min to 5°C / min; and / or, In the step of increasing the temperature from the second temperature to the third temperature, the heating rate is 5°C / min to 10°C / min; and / or, In the step of increasing the temperature from the third temperature to the fourth temperature, the heating rate is 10° C. / min to 15° C. / min.

5. The method for preparing the multi-level porous ceramic according to claim 1, characterized in that: The skeleton powder includes at least one of quartz powder, aluminum silicate and talc; and / or, The pore-forming agent comprises at least one of polystyrene microspheres and methyl methacrylate; and / or, The adhesive comprises at least one of carboxymethyl cellulose and ethyl cellulose; and / or, The solvent includes at least one of pinol and ethanol.

6. The method for preparing the multi-level porous ceramic according to claim 5, characterized in that: The skeleton powder is selected from quartz powder, aluminum silicate, calcium carbonate, and talc, the pore-forming agent is polystyrene microspheres, the adhesive is ethyl cellulose, and the solvent is ethanol and pinol. The weight ratio of the quartz powder to the first mixture is 25% to 30%, the weight ratio of the aluminum silicate to the first mixture is 5% to 10%, the weight ratio of the calcium carbonate to the first mixture is 1% to 2.5%, the weight ratio of the talc to the first mixture is 3% to 5%, the weight ratio of the polystyrene microspheres to the first mixture is 20% to 25%, the weight ratio of the ethyl cellulose to the first mixture is 2% to 3%, the weight ratio of the pinol alcohol to the first mixture is 12% to 18%, and the weight ratio of the ethanol to the first mixture is 20% to 25%.

7. The method for preparing the multi-level porous ceramic according to claim 1, characterized in that: The step of mixing the skeleton powder, the pore-forming agent, the adhesive and the solvent to form a first mixture comprises: Adding the skeleton powder, the pore-forming agent, the adhesive and the solvent into a stirring device; immersing a stirring device in water, starting the stirring device, and sealing and stirring to form a first mixture; Wherein, the temperature of the water is 55°C to 65°C; and / or, The sealed stirring time is 3h to 6h.

8. A multi-level porous ceramic, characterized in that: The multi-level porous ceramic is prepared by the method for preparing the multi-level porous ceramic according to any one of claims 1 to 7.

9. The multi-level porous ceramic according to claim 8, characterized in that: The multi-level porous ceramic is provided with internal through holes and surface through holes, the surface through holes connect the internal through holes with the external environment, the pore diameter of the surface through holes is 15 microns to 35 microns, and the pore diameter of the internal through holes is 100 microns to 1000 microns.

10. An atomizer core, characterized in that: The components of the atomizer core include the multi-level porous ceramic according to any one of claims 8 to 9; or, the components of the atomizer core include the multi-level porous ceramic prepared by the preparation method of the multi-level porous ceramic according to any one of claims 1 to 7.