Method for preparing silicon fertilizer from Portland cement construction waste and prepared silicon fertilizer
Through the combination of silicate cement construction waste and coal gangue, calcium carbonate and alkali, high-performance silicon fertilizer was prepared, which solved the problem of dense particles and small porosity of silicon fertilizer, improved the effective silicon content and specific surface area, and achieved the realization of Efficient resource utilization of construction waste.
Patent Information
- Application Number
- CN202310516507.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to effectively use silicate cement construction waste to prepare high-performance silicon fertilizers, resulting in dense particles, small porosity, and low effective silicon content, which cannot meet the requirements for use of silicon fertilizers.
Using the combination of silicate cement construction waste with coal gangue, calcium carbonate and alkali, the porous high-capacity calcium silicate and sodium silicate are formed through crushing, mixing, granulating, drying and baking activation. Properties of silicon fertilizers can improve the specific surface area and effective silicon content of silicon fertilizers.
The effective silicon content of silicon fertilizer is increased to 20-36 wt%, the specific surface area is 40-100m2/g, and the performance is better than conventional methods, while the resource utilization of construction waste is realized.
Smart Images

Figure BDA0004219364730000041 
Figure BDA0004219364730000071 
Figure BDA0004219364730000081
Abstract
Description
Technical Field
[0001] The invention belongs to the field of silicon fertilizer preparation, and relates to a method for preparing silicon fertilizer from silicate cement construction waste and the prepared silicon fertilizer. Background Art
[0002] With the acceleration of urbanization and industrialization in my country, the annual urban construction waste mainly composed of silicate cement generated by new construction, demolition and renovation has reached 1.55-2.4 billion tons, accounting for about 40% of urban solid waste. At present, the resource utilization rate of construction waste is less than 10%. Most of the construction waste is not treated and is directly transported to the suburbs for open-air stacking or landfill. Most of these construction wastes are difficult to degrade. Using traditional methods to treat them will not only occupy land, affect the city appearance and environmental sanitation, damage the ecological environment, cause serious waste of resources, but also pollute water and air.
[0003] The "Guidelines for the Priority Development of Key Areas of High-tech Industrialization in my country" clearly lists "recycling technology and equipment for waste concrete and various construction waste residues" as advanced manufacturing technology; and emphasizes "actively developing resource-based technologies for the production of building materials using waste residues" and "it is imperative to develop industrialized technologies and equipment that have a wide range of applications, can handle large amounts or a variety of solid wastes, have advanced technologies, low processing costs, and can be used as renewable resources."
[0004] How to recycle or harmlessly treat construction waste, which is mainly composed of silicate cement, is an important environmental issue and a problem that must be solved in the process of urban development. Portland cement is an indispensable raw material in concrete buildings. The common treatment method for these construction wastes is to use them as cement recycled aggregate or as building foundations for landfill. However, with the increase in demolition volume and the rapid urbanization process, these methods can no longer meet the needs of the rapid development of cities, and the cost of producing cement from other raw materials is much lower than the cost of recycling construction waste.
[0005] CN113321230 B discloses a method for preparing aluminum oxide and silicon fertilizer using fly ash, the steps comprising: mixing fly ash with ammonium sulfate and ammonium bicarbonate for reaction, solid-liquid separation, introducing NH3 into the filtrate to obtain basic ammonium aluminum carbonate solid; mixing the filter residue with calcium hydroxide, activating it by microwave treatment, and obtaining mixed silicon fertilizer.
[0006] CN109928782 A discloses a method for preparing silicon fertilizer from coal gangue, which comprises the following steps: testing of coal gangue raw materials, crushing of raw materials, batching, mixing, forming, thermal activation, quenching, drying, pulverizing and the like.
[0007] CN114956872 A discloses a method for preparing silicon fertilizer by activating coal gangue, and specifically relates to a technology for preparing silicon fertilizer by using organic solid waste + coal gangue.
[0008] At present, there are few reports on the preparation of silicon fertilizer using silicate cement construction waste. Summary of the invention
[0009] In order to solve the problem of recycling construction waste mainly composed of silicate cement, according to the characteristics of construction waste, if silicate cement construction waste is prepared into silicon fertilizer, the silicon fertilizer can be used to increase crop yields and can also be used for urban landscaping, so as to realize the recycling process of construction raw materials produced from nature, and then returned to nature after resource treatment.
[0010] Since silicate cement construction waste is the product of high-temperature roasting, if it is made into silicon fertilizer using conventional silicon fertilizer preparation methods, there are problems such as dense silicon fertilizer particles, small porosity, and inability to fully release effective silicon. Therefore, the content of effective silicon in the prepared silicon fertilizer is low and does not meet the use requirements of silicon fertilizer.
[0011] In order to realize the resource utilization of silicate cement construction waste and solve the problems of low porosity and poor fertilizer efficiency of silicon fertilizer prepared from silicate cement construction waste using conventional silicon fertilizer preparation methods, the present invention provides a method for preparing silicon fertilizer from silicate cement construction waste.
[0012] The principle of the present invention is as follows: silicate cement mainly contains substances such as dicalcium silicate and tricalcium silicate, with a content of up to 60-70wt%, and the content of silicon dioxide therein reaches 15-40wt%, which is a good raw material for preparing silicon fertilizer. The present invention utilizes the characteristics of silicate cement being rich in a large amount of water-soluble silicon, and is assisted by coal gangue, calcium carbonate and alkali activation to prepare porous high-performance silicon fertilizer rich in a large amount of soluble silicon such as calcium silicate and sodium silicate. Moreover, the voids formed after the combustion of organic matter in the coal gangue and the voids obtained by the decomposition of calcium carbonate to produce CO2 can make the silicon fertilizer particles form a porous medium, increase the porosity (i.e., specific surface area), and further increase the effective silicon content in the silicon fertilizer.
[0013] The process flow chart of the present invention for preparing silicon fertilizer is as follows Figure 1 shown.
[0014] Specifically, the present invention provides a method for preparing silicon fertilizer from silicate cement construction waste, comprising the following steps:
[0015] (1) Preparing a mixture of silicate cement construction waste and coal gangue: taking silicate cement construction waste and coal gangue and crushing them separately, mixing the crushed silicate cement construction waste and the crushed coal gangue, and crushing them again to obtain a raw material mixture 1;
[0016] (2) preparing an activator mixture: taking a calcium carbonate block, crushing it, and then mixing it with alkali to obtain an activator mixture 2;
[0017] (3) Raw material mixing: the raw material mixture 1 and the activator mixture 2 are mixed, and 15-25 wt% of water (for example, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, or a value or range between any two of these values) is added to the raw material mixture 1 and the activator mixture 2, and the mixture is mixed to obtain a mixture 3;
[0018] (4) Granulation: Granulating the mixed material 3 to obtain fertilizer granules;
[0019] (5) Drying: Drying the prepared fertilizer particles;
[0020] (6) Calcination and activation: Calcination and activation of the dried fertilizer particles, cooling the temperature to room temperature after calcination to obtain granular silicon fertilizer;
[0021] Wherein, the weight ratio of the silicate cement construction waste, the coal gangue, the calcium carbonate and the alkali is 1:(0.5-1.5):(0.375-1):(0.05-0.4);
[0022] The SiO2 content of the silicate cement construction waste is 15-40wt%, preferably 18-25wt%, for example, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, or a value or range of SiO2 between any two of these values, for example, 20.9wt% SiO2;
[0023] The SiO2 content of the coal gangue is 35-43wt%, for example, 35wt%, 36wt%, 37wt%, 38wt%, 39wt%, 40wt%, 41wt%, 42wt%, 43wt%, or a value or range of SiO2 between any two of these values;
[0024] The normal temperature may be 15-25°C.
[0025] In some embodiments, in the above method, the silicate cement construction waste may contain the following main components: 37-60wt% of tricalcium silicate, 15-37wt% of dicalcium silicate, 7-15wt% of tricalcium aluminate, 10-18wt% of tetracalcium aluminoferrite, wherein the content of SiO2 may be 18-25wt%.
[0026] In some embodiments, in any of the above methods, the gangue may contain the following main components: 20-35wt% organic matter, 35-43wt% SiO2, 14-28wt% Al2O3, 2.3-10.5wt% Fe2O3, 0.4-2.3wt% CaO, and 0.5-2.5wt% MgO.
[0027] In some embodiments, in any of the above methods, in step (1), the silicate cement construction waste and coal gangue are crushed to a particle size of less than 3 mm.
[0028] In some embodiments, in any of the above methods, in step (1), the crushed silicate cement construction waste and the crushed coal gangue are mixed and then crushed again to a particle size of less than 0.075 mm.
[0029] In some embodiments, in any of the above methods, in step (2), the calcium carbonate blocks are crushed to a particle size of less than 0.075 mm.
[0030] In some embodiments, in any of the above methods, in step (2), the base is selected from one or more of potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, potassium bicarbonate and sodium bicarbonate.
[0031] In some embodiments, in any of the above methods, in step (4), the particle size of the fertilizer particles is less than 3 mm.
[0032] In some embodiments, in any of the above methods, in step (4), the drying is any commonly used drying means, such as oven drying.
[0033] In some embodiments, in any of the methods described above, in step (6), the calcination conditions are as follows: the calcination temperature is 700-1000°C (for example, 700°C, 800°C, 900°C, 1000°C, or a temperature in a numerical value or range between any two of these values), and the calcination time is 1-3 hours (for example, 1 hour, 2 hours, 3 hours, or a time in a numerical value or range between any two of these values).
[0034] In some embodiments, in any of the above methods, the weight ratio of the silicate cement construction waste, the coal gangue, the calcium carbonate, and the alkali is 1:(1-1.5):(0.375-1):(0.05-0.4), preferably 1:1:(0.5-1):(0.1-0.4).
[0035] In some embodiments, in any of the above methods, the weight ratio of the calcium carbonate to the alkali is 5:1.
[0036] In some embodiments, in any of the above methods, the effective silicon content of the silicon fertilizer is greater than 20 wt %.
[0037] In some embodiments, in any of the above methods, the effective silicon content of the silicon fertilizer is 20-36wt%, preferably 23-36wt%, and more preferably 30-36wt%.
[0038] The present invention also provides silicon fertilizer prepared by any of the above methods.
[0039] The specific surface area of the silicon fertilizer prepared by using silicate cement construction waste is 40-100m 2 / g, and the effective silicon content is 20-36wt%. The silicon fertilizer prepared by the present invention using silicate cement construction waste has better performance than the conventional method, and at the same time realizes the resource utilization of construction waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The present invention is a process flow chart for preparing silicon fertilizer.
[0041] Figure 2 This is the XRD pattern of the silicon fertilizer prepared in Example 2 of the present invention.
[0042] Figure 3 The effect of the weight ratio of alkali to calcium carbonate on the specific surface area and effective silicon content of silicon fertilizer. DETAILED DESCRIPTION
[0043] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0044] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0045] The present invention will be further described below in conjunction with specific examples. It should be understood that the following examples are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0046] The main components of the silicate cement construction waste used in the following examples are shown in Table 1, and the SiO2 content is 20.9wt%.
[0047] Table 1
[0048] Components Tricalcium silicate Dicalcium Silicate Tricalcium aluminate Tetracalcium aluminoferrite Content (wt%) 53.1 19.9 12.4 14.6
[0049] The coal gangue used in the following examples comes from a coal mine, and its main components are shown in Table 2.
[0050] Table 2
[0051]
[0052] In the following examples, 1 part by weight means 1 kg.
[0053] Specific surface area detection method of silicon fertilizer: GB / T 8074-2008 Determination method of specific surface area of cement. Blaine method.
[0054] Detection method for effective silicon content in silicon fertilizer: NY / T 797-2004 silicon fertilizer.
[0055] Example 1
[0056] 1. Prepare a mixture of silicate cement construction waste and coal gangue: take 1 part by weight of silicate cement construction waste and put it into a crusher to crush it to a particle size of less than 3 mm for later use, take 0.5 part by weight of coal gangue and put it into a crusher to crush it to a particle size of less than 3 mm for later use, mix and stir the crushed silicate cement construction waste and the crushed coal gangue, put them into the crusher again and crush them to a particle size of less than 0.075 mm to obtain a raw material mixture 1.
[0057] 2. Preparation of activator mixture: 0.75 parts by weight of calcium carbonate block is put into a crusher and crushed to a particle size of less than 0.075 mm, and mixed with 0.15 parts by weight of sodium hydroxide to obtain activator mixture 2.
[0058] 3. Raw material mixing: Mix the raw material mixture 1 and the activator mixture 2 evenly, add 20 wt % of water accounting for the total amount of the raw material mixture 1 and the activator mixture 2, stir and mix evenly, and obtain mixture 3.
[0059] 4. Granulation: Add the mixture 3 into a high-speed granulator to prepare fertilizer granules with a particle size of less than 3 mm.
[0060] 5. Drying: Put the prepared fertilizer particles into the dryer for drying.
[0061] 6. Calcination and activation: Place the dried fertilizer granules into a calcination furnace for calcination and activation. The calcination temperature is 800°C and the calcination time is 2 hours. After calcination, cool down to room temperature to obtain granular silicon fertilizer.
[0062] Example 2
[0063] 1. Prepare a mixture of silicate cement construction waste and coal gangue: take 1 part by weight of silicate cement construction waste and put it into a crusher to crush it to a particle size of less than 3 mm for later use; take 1 part by weight of coal gangue and put it into a crusher to crush it to a particle size of less than 3 mm for later use; mix and stir the crushed silicate cement construction waste and the crushed coal gangue, put them into the crusher again and crush them to a particle size of less than 0.075 mm to obtain a raw material mixture 1.
[0064] 2. Preparation of activator mixture: 0.75 parts by weight of calcium carbonate block is put into a crusher and crushed to a particle size of less than 0.075 mm, and mixed with 0.15 parts by weight of sodium hydroxide to obtain activator mixture 2.
[0065] 3. Raw material mixing: Mix the raw material mixture 1 and the activator mixture 2 evenly, add 20 wt % of water accounting for the total amount of the raw material mixture 1 and the activator mixture 2, stir and mix evenly, and obtain mixture 3.
[0066] 4. Granulation: Add the mixture 3 into a high-speed granulator to prepare fertilizer granules with a particle size of less than 3 mm.
[0067] 5. Drying: Put the prepared fertilizer particles into the dryer for drying.
[0068] 6. Calcination and activation: Place the dried fertilizer granules into a calcination furnace for calcination and activation. The calcination temperature is 800°C and the calcination time is 2 hours. After calcination, cool down to room temperature to obtain granular silicon fertilizer.
[0069] Example 3
[0070] 1. Prepare a mixture of silicate cement construction waste and coal gangue: take 1 part by weight of silicate cement construction waste and put it into a crusher to crush it to a particle size of less than 3 mm for later use, take 1.5 parts by weight of coal gangue and put it into a crusher to crush it to a particle size of less than 3 mm for later use, mix and stir the crushed silicate cement construction waste and the crushed coal gangue, put them into the crusher again and crush them to a particle size of less than 0.075 mm to obtain a raw material mixture 1.
[0071] 2. Preparation of activator mixture: 0.75 parts by weight of calcium carbonate block is put into a crusher and crushed to a particle size of less than 0.075 mm, and mixed with 0.15 parts by weight of sodium hydroxide to obtain activator mixture 2.
[0072] 3. Raw material mixing: Mix the raw material mixture 1 and the activator mixture 2 evenly, add 20 wt % of water accounting for the total amount of the raw material mixture 1 and the activator mixture 2, stir and mix evenly, and obtain mixture 3.
[0073] 4. Granulation: Add the mixture 3 into a high-speed granulator to prepare fertilizer granules with a particle size of less than 3 mm.
[0074] 5. Drying: Put the prepared fertilizer particles into the dryer for drying.
[0075] 6. Calcination and activation: Place the dried fertilizer granules into a calcination furnace for calcination and activation. The calcination temperature is 800°C and the calcination time is 2 hours. After calcination, cool down to room temperature to obtain granular silicon fertilizer.
[0076] Example 4
[0077] According to the method of Example 2, the only difference is that step 2 is replaced by the following steps to prepare granular silicon fertilizer:
[0078] 2. Preparation of activator mixture: 0.375 parts by weight of calcium carbonate block is put into a crusher and crushed to a particle size of less than 0.075 mm, and mixed with 0.075 parts by weight of sodium hydroxide to obtain activator mixture 2.
[0079] Example 5
[0080] According to the method of Example 2, the only difference is that step 2 is replaced by the following steps to prepare granular silicon fertilizer:
[0081] 2. Preparation of activator mixture: 0.5 parts by weight of calcium carbonate block is put into a crusher and crushed to a particle size of less than 0.075 mm, and mixed with 0.1 parts by weight of sodium hydroxide to obtain activator mixture 2.
[0082] Example 6
[0083] According to the method of Example 2, the only difference is that step 2 is replaced by the following steps to prepare granular silicon fertilizer:
[0084] 2. Preparation of activator mixture: 1 part by weight of calcium carbonate block is put into a crusher and crushed to a particle size of less than 0.075 mm, and mixed evenly with 0.2 parts by weight of sodium hydroxide to obtain activator mixture 2.
[0085] Example 7
[0086] According to the method of Example 2, the only difference is that step 2 is replaced by the following steps to prepare granular silicon fertilizer:
[0087] 2. Preparation of activator mixture: 0.85 parts by weight of calcium carbonate block is put into a crusher and crushed to a particle size of less than 0.075 mm, and mixed with 0.05 parts by weight of sodium hydroxide to obtain activator mixture 2.
[0088] Example 8
[0089] According to the method of Example 2, the only difference is that step 2 is replaced by the following steps to prepare granular silicon fertilizer:
[0090] 2. Preparation of activator mixture: 0.8 parts by weight of calcium carbonate block is put into a crusher and crushed to a particle size of less than 0.075 mm, and mixed with 0.1 parts by weight of sodium hydroxide to obtain activator mixture 2.
[0091] Example 9
[0092] According to the method of Example 2, the only difference is that step 2 is replaced by the following steps to prepare granular silicon fertilizer:
[0093] 2. Preparation of activator mixture: 0.7 parts by weight of calcium carbonate block is put into a crusher and crushed to a particle size of less than 0.075 mm, and mixed with 0.2 parts by weight of sodium hydroxide to obtain activator mixture 2.
[0094] Example 10
[0095] According to the method of Example 2, the only difference is that step 2 is replaced by the following steps to prepare granular silicon fertilizer:
[0096] 2. Preparation of activator mixture: 0.6 parts by weight of calcium carbonate block is put into a crusher and crushed to a particle size of less than 0.075 mm, and mixed with 0.3 parts by weight of sodium hydroxide to obtain activator mixture 2.
[0097] Embodiment 11
[0098] According to the method of Example 2, the only difference is that step 2 is replaced by the following steps to prepare granular silicon fertilizer:
[0099] 2. Preparation of activator mixture: 0.5 parts by weight of calcium carbonate block is put into a crusher and crushed to a particle size of less than 0.075 mm, and mixed with 0.4 parts by weight of sodium hydroxide to obtain activator mixture 2.
[0100] Example 12
[0101] According to the method of Example 2, the only difference is that step 6 is replaced by the following steps to prepare granular silicon fertilizer:
[0102] 6. Calcination and activation: Place the dried fertilizer granules into a calcination furnace for calcination and activation. The calcination temperature is 700°C and the calcination time is 2 hours. After calcination, cool down to room temperature to obtain granular silicon fertilizer.
[0103] Example 13
[0104] According to the method of Example 2, the only difference is that step 6 is replaced by the following steps to prepare granular silicon fertilizer:
[0105] 6. Calcination and activation: Place the dried fertilizer granules into a calcination furnace for calcination and activation. The calcination temperature is 900°C and the calcination time is 2 hours. After calcination, cool down to room temperature to obtain granular silicon fertilizer.
[0106] Embodiment 14
[0107] According to the method of Example 2, the only difference is that step 6 is replaced by the following steps to prepare granular silicon fertilizer:
[0108] 6. Calcination and activation: Place the dried fertilizer granules into a calcination furnace for calcination and activation. The calcination temperature is 1000°C and the calcination time is 2 hours. After calcination, cool down to room temperature to obtain granular silicon fertilizer.
[0109] Embodiment 15
[0110] According to the method of Example 2, the only difference is that step 6 is replaced by the following steps to prepare granular silicon fertilizer:
[0111] 6. Calcination and activation: Place the dried fertilizer granules into a calcination furnace for calcination and activation. The calcination temperature is 800°C and the calcination time is 1 hour. After calcination, cool down to room temperature to obtain granular silicon fertilizer.
[0112] Example 16
[0113] According to the method of Example 2, the only difference is that step 6 is replaced by the following steps to prepare granular silicon fertilizer:
[0114] 6. Calcination and activation: Place the dried fertilizer granules into a calcination furnace for calcination and activation. The calcination temperature is 800°C and the calcination time is 3 hours. After calcination, cool down to room temperature to obtain granular silicon fertilizer.
[0115] Comparative Example 1
[0116] Granular silicon fertilizer is prepared according to the method of Example 2, except that step 2 is not performed and step 3 is replaced by the following steps:
[0117] 3. Add 20 wt% of water to the raw material mixture 1, stir and mix evenly to obtain mixture 3.
[0118] Comparative Example 2
[0119] According to the method of Example 2, the only difference is that step 1 is replaced by the following steps to prepare granular silicon fertilizer:
[0120] 1. Preparation of Portland cement construction waste raw material: 2.7 parts by weight of Portland cement construction waste was put into a crusher and crushed to a particle size of less than 0.075 mm to obtain raw material 1.
[0121] Comparative Example 3
[0122] According to the method of Example 2, the only difference is that step 1 is replaced by the following steps to prepare granular silicon fertilizer:
[0123] 1. Preparation of coal gangue raw material: 1.59 parts by weight of coal gangue was put into a crusher and crushed to a particle size of less than 0.075 mm to obtain raw material 1.
[0124] In the examples and comparative examples, the weight of each component and the specific surface area and effective silicon content of the prepared silicon fertilizer are shown in Table 3.
[0125] Table 3
[0126]
[0127]
[0128] The XRD pattern of the silicon fertilizer prepared in Example 2 is as follows: Figure 2 XRD characterization shows that after calcination and activation, a large amount of soluble calcium silicate and sodium silicate are generated, which are the main sources of effective silicon.
[0129] The specific surface area and effective silicon content of the silicon fertilizers prepared in Examples 2 and 7-11 are as follows: Figure 3 shown. Figure 3 The effect of alkali / calcium carbonate on the specific surface area and effective silicon content of silicon fertilizer is shown, indicating that when alkali / calcium carbonate ≥ 0.2, the effective silicon and specific surface area no longer increase significantly.
[0130] In Comparative Example 1, no activator was added, and the specific surface area of the prepared silicon fertilizer was very low, the effective silicon could not be fully released, and the effective silicon content was far lower than the national standard content of 20wt% for silicon fertilizer, which did not meet the use requirements of silicon fertilizer.
[0131] Comparative Example 2 adopts a conventional silicon fertilizer preparation method, and an activator is added to silicate cement construction waste to prepare silicon fertilizer. This silicon fertilizer also has the problem that the effective silicon cannot be fully released due to the low specific surface area. The effective silicon content is only about 10wt%, which is far lower than the national standard content of 20wt% for effective silicon fertilizer, and does not meet the use requirements of silicon fertilizer.
[0132] The present invention has been described with reference to the embodiments and examples. However, the present invention is not limited to the aspects described in the above embodiments and examples, and various modifications may be made. However, it should be understood that it is possible for those skilled in the art to make various modifications and equivalent substitutions to the present invention without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited to the specific embodiments described herein. More specifically, the scope of protection of the present invention is defined by the appended claims.
Claims
1. A method for preparing silicon fertilizer from silicate cement construction waste, comprising the following steps: (1) Preparing a mixture of silicate cement construction waste and coal gangue: taking silicate cement construction waste and coal gangue and crushing them separately, mixing the crushed silicate cement construction waste and the crushed coal gangue, and crushing them again to obtain a raw material mixture 1; (2) preparing an activator mixture: taking a calcium carbonate block, crushing it, and then mixing it with alkali to obtain an activator mixture 2; (3) Raw material mixing: the raw material mixture 1 and the activator mixture 2 are mixed, and water accounting for 15-25 wt % of the total amount of the raw material mixture 1 and the activator mixture 2 is added, and mixed to obtain a mixture 3; (4) Granulation: Granulating the mixed material 3 to obtain fertilizer granules; (5) Drying: Drying the prepared fertilizer particles; (6) Calcination and activation: Calcination and activation of the dried fertilizer particles, cooling the temperature to room temperature after calcination to obtain granular silicon fertilizer; in, The weight ratio of the silicate cement construction waste, the coal gangue, the calcium carbonate and the alkali is 1:(0.5-1.5):(0.375-1):(0.05-0.4); The SiO2 content of the silicate cement construction waste is 15-40wt%; The SiO2 content of the coal gangue is 35-43wt%.
2. The method according to claim 1, characterized in that: In step (1), the silicate cement construction waste and coal gangue are crushed to a particle size of less than 3 mm respectively; and / or In step (1), the crushed silicate cement construction waste and the crushed coal gangue are mixed and then crushed again to a particle size of less than 0.075 mm.
3. The method according to claim 1 or 2, characterized in that: In step (2), the calcium carbonate blocks are crushed to a particle size of less than 0.075 mm.
4. The method according to any one of claims 1 to 3, characterized in that: In step (2), the base is selected from one or more of potassium hydroxide, sodium hydroxide, potassium carbonate, sodium carbonate, potassium bicarbonate and sodium bicarbonate.
5. The method according to any one of claims 1 to 4, characterized in that: In step (4), the particle size of the fertilizer particles is less than 3 mm.
6. The method according to any one of claims 1 to 5, characterized in that: In step (6), the calcination conditions are: calcination temperature 700-1000° C., calcination time 1-3 hours.
7. The method according to any one of claims 1 to 6, characterized in that: The weight ratio of the silicate cement construction waste, the coal gangue, the calcium carbonate and the alkali is 1:(1-1.5):(0.375-1):(0.05-0.4).
8. The method according to any one of claims 1 to 7, characterized in that: The weight ratio of the calcium carbonate to the alkali is 5:
1.
9. The method according to any one of claims 1 to 8, characterized in that: The effective silicon content of the silicon fertilizer is greater than 20wt%.