Acrylic resin as well as preparation method and application thereof
By adjusting the component ratio and structure of acrylic resin, an acrylic resin with a balance of rigidity and toughness was synthesized, which solved the problems of insufficient wear resistance, acid resistance and aging resistance of acrylic coatings and improved the overall performance of the coatings.
Patent Information
- Application Number
- CN202411171718.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-12
AI Technical Summary
Existing acrylic coatings are insufficient in terms of abrasion resistance, acid resistance, and aging resistance, making it difficult to meet the application requirements of automotive coatings.
By controlling the proportions of acrylic acid, 2-furanacrylic acid, and cinnamic acid, as well as the amounts of acrylic monomers and oleylamine, an acrylic resin with flexible alkyl branches, a rigid benzene ring structure, and a furan group with high tension was synthesized, thereby regulating its rigidity-toughness balance and structural stability.
It improves the abrasion resistance, acid resistance, and aging resistance of acrylic coatings, and enhances the environmental adaptability of the coatings.
Smart Images

Figure BDA0005009469420000041 
Figure BDA0005009469420000042 
Figure BDA0005009469420000051
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, and more specifically to an acrylic resin and a preparation method and application thereof. Background Art
[0002] Acrylic resins are often used to prepare coatings for various fields due to their advantages such as light color and transparency, such as acrylic coatings for the automotive field. In daily use, cars often rub against various objects. In order to reduce damage to cars, acrylic coatings as protective covers for cars should have wear resistance. Due to environmental pollution, acid rain has become more frequent. In order to resist the damage of acid rain, acrylic coatings should be acid-resistant. In addition, in daily use, cars are often exposed to harsh environments such as scorching sun and heavy rain. In order to extend the service life of the coating, acrylic coatings should be aging-resistant.
[0003] Therefore, it is of great significance to develop an acrylic resin that can simultaneously improve the wear resistance, acid resistance and aging resistance of acrylic coatings. Summary of the invention
[0004] The purpose of the present invention is to solve the problem of improving the wear resistance, acid resistance and aging resistance of acrylic paint, and to provide an acrylic resin and a preparation method and application thereof.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] In a first aspect, the present invention provides an acrylic resin, wherein the raw materials thereof include the following components in parts by weight:
[0007] 80-120 parts of acrylic monomer, 5-40 parts of oleylamine, 3-8 parts of initiator, 15-25 parts of solvent;
[0008] The acrylic acid monomers are acrylic acid, 2-furan acrylic acid and cinnamic acid in a weight ratio of 10:(2-8):(3-10).
[0009] The acrylic resin synthesized by the invention by controlling the usage ratio of acrylic acid, 2-furan acrylic acid and cinnamic acid in acrylic monomers and the usage of acrylic monomers and oleylamine can simultaneously improve the wear resistance, acid resistance and aging resistance of acrylic paint.
[0010] Specifically, the acrylic resin of the present invention has a flexible alkyl side chain and a rigid benzene ring structure, as well as a furan group with high tension, which makes the acrylic resin not only have the characteristics of rigidity and toughness balance, but also have a stable structure and buffering properties against environmental changes, which is beneficial to improving the wear resistance, acid resistance and aging resistance of the acrylic coating prepared using the acrylic resin.
[0011] The invention can adjust the amount of flexible alkyl side chains, rigid benzene ring structures and furan groups with large tension in acrylic resin by controlling the usage ratio of acrylic acid, 2-furan acrylic acid and cinnamic acid, as well as the usage of acrylic monomers and oleylamine, thereby improving the rigid-toughness balance property, structural stability and buffering property against environmental changes of the acrylic resin, and ultimately being beneficial to improving the wear resistance, acid resistance and aging resistance of acrylic coating prepared by using the acrylic resin.
[0012] Preferably, the weight ratio of acrylic acid, 2-furanacrylic acid and cinnamic acid is 10:5:5.
[0013] Preferably, the weight proportion of the oleylamine is 15-25 parts.
[0014] Preferably, the initiator is at least one of a peroxide compound initiator and an azo initiator.
[0015] More preferably, the peroxide compound initiator is at least one of hydrogen peroxide, ammonium persulfate and potassium persulfate.
[0016] More preferably, the azo initiator is at least one of azobisisobutyronitrile and azobisisoheptanenitrile.
[0017] Preferably, the solvent is at least one of ethanol, water and isopropanol.
[0018] More preferably, the solvent is ethanol and water in a weight ratio of 1:(0.2-1).
[0019] In a second aspect, the present invention provides a method for preparing an acrylic resin, comprising the following steps:
[0020] The components of the acrylic resin raw material are mixed and heated to react to obtain the acrylic resin.
[0021] Preferably, the temperature of the heating reaction is 70-90°C.
[0022] Preferably, the heating reaction time is 3-8h.
[0023] In a third aspect, the present invention provides an application of an acrylic resin in a coating.
[0024] In a fourth aspect, the present invention provides an acrylic paint comprising the following components in parts by weight:
[0025] 75-100 parts of acrylic resin, 10-20 parts of curing agent, 1-5 parts of film-forming aid.
[0026] Preferably, the curing agent is a water-based isocyanate curing agent, such as Bayhydur 304 produced by Bayer (Covestro).
[0027] Preferably, the film-forming aid is at least one of ethylene glycol n-butyl ether, propylene glycol ethyl ether, ethylene glycol, propylene glycol, and hexylene glycol.
[0028] Preferably, the acrylic paint further comprises an auxiliary agent.
[0029] More preferably, the weight proportion of the auxiliary agent is 1-10 parts.
[0030] More preferably, the auxiliary agent includes at least one of a leveling agent, a defoaming agent and a wetting agent.
[0031] In the present invention, the leveling agent, defoaming agent and wetting agent commonly used in the art can be used in the present invention.
[0032] In a fifth aspect, the present invention provides a method for preparing an acrylic paint, comprising the following steps: mixing the components to obtain the acrylic paint.
[0033] In a sixth aspect, the present invention provides a use of acrylic paint in an automobile.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] The acrylic resin synthesized by the invention by controlling the usage ratio of acrylic acid, 2-furan acrylic acid and cinnamic acid in acrylic monomers and the usage of acrylic monomers and oleylamine can simultaneously improve the wear resistance, acid resistance and aging resistance of acrylic paint.
[0036] Specifically, the acrylic resin of the present invention has a flexible alkyl side chain and a rigid benzene ring structure, as well as a furan group with high tension, which makes the acrylic resin not only have the characteristics of rigidity and toughness balance, but also have a stable structure and buffering properties against environmental changes, which is beneficial to improving the wear resistance, acid resistance and aging resistance of the acrylic coating prepared using the acrylic resin.
[0037] The invention can adjust the amount of flexible alkyl side chains, rigid benzene ring structures and furan groups with large tension in acrylic resin by controlling the usage ratio of acrylic acid, 2-furan acrylic acid and cinnamic acid, as well as the usage of acrylic monomers and oleylamine, thereby improving the rigid-toughness balance property, structural stability and buffering property against environmental changes of the acrylic resin, and ultimately being beneficial to improving the wear resistance, acid resistance and aging resistance of acrylic coating prepared by using the acrylic resin. DETAILED DESCRIPTION
[0038] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0039] In each application example of the present invention and the comparative application example, the use of the reagents is as follows:
[0040] Water-based isocyanate curing agent, Bayhydur304, Bayer (Covestro);
[0041] Defoamer, BYK-019, BYK.
[0042] Example 1
[0043] This embodiment provides an acrylic resin, the raw materials of which include the following components in parts by weight:
[0044] 100 parts of acrylic monomer, 20 parts of oleylamine, 5 parts of initiator azobisisobutyronitrile, 20 parts of solvent;
[0045] The acrylic acid monomers are acrylic acid, 2-furan acrylic acid and cinnamic acid in a weight ratio of 10:5:5;
[0046] The solvent is anhydrous ethanol and water in a weight ratio of 1:1;
[0047] The preparation method of the acrylic resin comprises the following steps:
[0048] The components of the acrylic resin raw material are mixed, heated to 80°C for reaction for 5 hours to obtain acrylic resin.
[0049] Examples 2-5 and Comparative Examples 1-4
[0050] Examples 2-5 and Comparative Examples 1-4 provide different acrylic resins, which differ from Example 1 in that the weight ratios of acrylic acid, 2-furan acrylic acid and cinnamic acid are different, and the rest are consistent with Example 1, as shown in the following table:
[0051] Table 1 Weight ratio of acrylic acid, 2-furan acrylic acid and cinnamic acid in Examples 1-5 and Comparative Examples 1-4
[0052]
[0053] Examples 6-11 and Comparative Examples 5-7
[0054] Examples 6-11 and Comparative Examples 5-7 provide different acrylic resins, which differ from Example 1 in that the amounts of acrylic monomer and oleylamine used are different, and the rest are consistent with Example 1, as shown in the following table:
[0055] Table 2 Amounts of acrylic monomer and oleylamine used in Examples 1, 6-11 and Comparative Examples 5-7
[0056]
[0057]
[0058] Example 12
[0059] This embodiment provides an acrylic resin, the raw materials of which include the following components in parts by weight:
[0060] 100 parts of acrylic monomer, 20 parts of oleylamine, 3 parts of initiator azobisisobutyronitrile, 15 parts of solvent;
[0061] The acrylic acid monomers are acrylic acid, 2-furan acrylic acid and cinnamic acid in a weight ratio of 10:5:5;
[0062] The solvent is anhydrous ethanol and water in a weight ratio of 1:0.2;
[0063] The preparation method of the acrylic resin comprises the following steps:
[0064] The components of the acrylic resin raw material are mixed, heated to 80°C for reaction for 5 hours to obtain acrylic resin.
[0065] Example 13
[0066] This embodiment provides an acrylic resin, the raw materials of which include the following components in parts by weight:
[0067] 100 parts of acrylic monomer, 20 parts of oleylamine, 8 parts of initiator azobisisobutyronitrile, 25 parts of solvent;
[0068] The acrylic acid monomers are acrylic acid, 2-furan acrylic acid and cinnamic acid in a weight ratio of 10:5:5;
[0069] The solvent is anhydrous ethanol and water in a weight ratio of 1:1;
[0070] The preparation method of the acrylic resin comprises the following steps:
[0071] The components of the acrylic resin raw material are mixed, heated to 80°C for reaction for 5 hours to obtain acrylic resin.
[0072] Application examples and comparative application examples
[0073] Application Example 1
[0074] This application example provides an acrylic paint, comprising the following components in parts by weight:
[0075] 90 parts of the acrylic resin of Example 1, 15 parts of an aqueous isocyanate curing agent, 3 parts of a film-forming aid propylene glycol ethyl ether, and 5 parts of a defoaming agent;
[0076] The preparation method of the acrylic paint comprises the following steps: mixing the components to obtain the acrylic paint.
[0077] Application Example 2-13
[0078] Application Examples 2-13 provide different acrylic coatings, which differ from Application Example 1 in that Application Examples 2-13 use the acrylic resins of Examples 2-13 to replace the acrylic resin of Example 1, and the rest are consistent with Application Example 1.
[0079] Comparative Application Examples 1-7
[0080] Comparative Application Examples 1-7 provide different acrylic coatings, which differ from Application Example 1 in that Comparative Application Examples 1-7 use acrylic resins of Comparative Examples 1-7 to replace the acrylic resin of Example 1, and the rest are consistent with Application Example 1.
[0081] Performance Testing
[0082] The performance tests of the acrylic paints of each application example and comparative application example are as follows:
[0083] (1) Adhesion test:
[0084] 35g of acrylic paint was applied on a 100mm*100mm*2mm tinplate plane and dried at 80℃ for 24h to obtain a test sample. The adhesion test was performed according to GB / T 9286-2021. The larger the adhesion level, the worse the adhesion of the acrylic paint.
[0085] (2) Wear resistance test:
[0086] 35g of acrylic paint was coated on a 100mm*100mm*2mm tinplate plane and dried at 80℃ for 24h to obtain a test sample. According to GB / T 1768-2006, the wear mass of the paint was measured (accurate to 0.1mg) under the conditions of a rubber grinding wheel load of 1000g and a test rotation number of 1000 revolutions. The greater the wear mass, the worse the wear resistance of the acrylic paint.
[0087] (3) Acid resistance test:
[0088] 35g of acrylic paint was coated on the flat surface of a 100mm*100mm*2mm tinplate, and dried at 80℃ for 24h to obtain a test sample. The acid resistance test was carried out according to the provisions of Method A of GB / T 9274-1988. The test sample was immersed in a 10% H2SO4 solution by mass for 40d, and the sample was taken out and wiped dry with filter paper. The paint film was visually observed under scattered sunlight, and discoloration and loss of gloss were allowed. The acid resistance was rated. The larger the grade, the worse the acid resistance of the acrylic paint, as follows:
[0089] Level 0: No abnormal paint film phenomena such as blistering, cracking, peeling, rusting, etc. occur on the surface of the sample;
[0090] Level 1: The area of abnormal paint film phenomena such as blistering, cracking, peeling, rusting, etc. on the sample surface accounts for 0-25% of the total surface area of the sample, and is not 0;
[0091] Level 2: The area of abnormal paint film phenomena such as blistering, cracking, peeling, rusting, etc. on the sample surface accounts for 25%-50% of the total surface area of the sample, but not 25%;
[0092] Level 3: The area of abnormal paint film phenomena such as blistering, cracking, peeling, rusting, etc. on the sample surface accounts for 50%-75% of the total surface area of the sample, but not 50%;
[0093] Level 4: The area of abnormal paint film phenomena such as blistering, cracking, peeling, rusting, etc. on the sample surface accounts for 75%-100% of the total surface area of the sample, but is not 75%.
[0094] (4) Aging resistance test:
[0095] 35g of acrylic paint was coated on a 100mm*100mm*2mm tinplate plane and dried at 80℃ for 24h to obtain a test sample. The sample was tested for 800h according to method B of GB / T 23987-2009. The aging resistance of the acrylic paint was graded according to Table 23 of GB / T1766-2008 "Evaluation of comprehensive aging performance grade of protective paint film". The larger the grade, the worse the aging resistance of the acrylic paint.
[0096] The experimental results are shown in the following table:
[0097] Table 3 Performance test results of nano silicon carbon negative electrode materials in various application examples and comparative application examples
[0098]
[0099]
[0100] As can be seen from Table 3, the acrylic resin synthesized by controlling the usage ratio of acrylic acid, 2-furan acrylic acid and cinnamic acid in the acrylic monomers, as well as the usage of acrylic monomers and oleylamine can simultaneously improve the wear resistance, acid resistance and aging resistance of acrylic coatings.
[0101] Specifically, the acrylic resin of the present invention has a flexible alkyl side chain and a rigid benzene ring structure, as well as a furan group with high tension, which makes the acrylic resin not only have the characteristics of rigidity and toughness balance, but also have a stable structure and buffering properties against environmental changes, which is beneficial to improving the wear resistance, acid resistance and aging resistance of the acrylic coating prepared using the acrylic resin.
[0102] It can be seen from Application Examples 1-11 and Comparative Application Examples 1-7 that the present invention can regulate the number of flexible alkyl side chains, rigid benzene ring structures and furan groups with high tension in acrylic resin by controlling the dosage ratio of acrylic acid, 2-furan acrylic acid and cinnamic acid, as well as the dosage of acrylic monomers and oleylamine, thereby improving the rigid-toughness balance characteristics, structural stability and buffering characteristics of the acrylic resin against environmental changes, which is ultimately beneficial to improving the wear resistance, acid resistance and aging resistance of acrylic coatings prepared using acrylic resin.
[0103] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. An acrylic resin, characterized in that The raw materials include the following components in parts by weight: 80-120 parts of acrylic monomer, 5-40 parts of oleylamine, 3-8 parts of initiator, 15-25 parts of solvent; The acrylic acid monomers are acrylic acid, 2-furan acrylic acid and cinnamic acid in a weight ratio of 10:(2-8):(3-10).
2. The acrylic resin according to claim 1, characterized in that Include at least one of the following (1)-(2): (1) The weight ratio of acrylic acid, 2-furan acrylic acid and cinnamic acid is 10:5:5; (2) The weight proportion of the oleylamine is 15-25 parts.
3. The acrylic resin according to claim 1, characterized in that Include at least one of the following (1)-(2): (1) The initiator is at least one of a peroxide compound initiator and an azo initiator; (2) The solvent is at least one of ethanol, water, and isopropanol.
4. The acrylic resin according to claim 3, characterized in that Including at least one of the following (1)-(3): (1) The peroxide compound initiator is at least one of hydrogen peroxide, ammonium persulfate, and potassium persulfate; (2) The azo initiator is at least one of azobisisobutyronitrile and azobisisoheptanenitrile; (3) The solvent is ethanol and water in a weight ratio of 1:(0.2-1).
5. The method for preparing the acrylic resin according to any one of claims 1 to 4, characterized in that: The steps include: The components of the acrylic resin raw material are mixed and heated to react to obtain the acrylic resin.
6. The method for preparing acrylic resin according to claim 5, characterized in that: The temperature of the heating reaction is 70-90°C.
7. Use of the acrylic resin according to any one of claims 1 to 4 in coatings.
8. An acrylic paint, characterized in that: The composition comprises the following components in parts by weight: 75-100 parts of the acrylic resin according to any one of claims 1-4, 10-20 parts of a curing agent, and 1-5 parts of a film-forming aid.
9. The acrylic paint according to claim 8, characterized in that: Including at least one of the following (1)-(3): (1) The curing agent is a water-based isocyanate curing agent; (2) The film-forming aid is at least one of ethylene glycol n-butyl ether, propylene glycol ethyl ether, ethylene glycol, propylene glycol, and hexylene glycol; (3) The acrylic paint further comprises an auxiliary agent, and the weight proportion of the auxiliary agent is 1-10 parts.
10. The method for preparing the acrylic paint according to any one of claims 8 to 9, characterized in that: The method comprises the following steps: mixing various components to obtain acrylic paint.