Polymethyl methacrylate / nano titanium dioxide composite material as well as preparation method and application thereof

By adding titanium and acid sources to PMMA and using ultrasound treatment and ultraviolet or thermal conditions during the polymerization process, uniformly dispersed nanotitanium dioxide particles are solved, and the problems of low ultraviolet absorption rate and difficulty in dispersing nanotitanium dioxide are achieved. It has high performance ultraviolet absorption and biocompatibility, and is suitable for biomedical materials such as artificial cornea.

CN118930711APending Publication Date: 2024-11-12SHANGHAI VISION SCIENCE ENGINEER MEDICAL EQUIPMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410991812.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing artificial corneal materials of polymethyl methacrylate (PMMA) do not have high UV absorption rate, and the uniform dispersion of nanotitanium dioxide in polymers is difficult, resulting in a decrease in UV absorption capacity and transparency, and a risk of toxicity.

Method used

By adding titanium sources, acid sources and initiators to PMMA, polymerization is carried out using sonication and ultraviolet or thermal conditions to form uniformly dispersed nanotitanium dioxide particles, ensuring their stable distribution in the polymer and improving the ultraviolet absorption capacity.

Benefits of technology

It achieves high-performance ultraviolet absorption capacity, avoids the agglomeration and toxicity risks of nanotitanium dioxide, maintains the transparency and biocompatibility of the material, and is suitable for biomedical materials such as artificial cornea.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930711A_ABST
    Figure CN118930711A_ABST
Patent Text Reader

Abstract

The invention discloses a polymethyl methacrylate / nano titanium dioxide composite material as well as a preparation method and application thereof. According to the method, a methyl methacrylate monomer is mixed with a titanium source, an acid source and a small amount of water, so that the acid source is uniformly distributed in the composite material through a copolymerization reaction with methyl methacrylate. Under the catalysis of an acid source, a titanium source reacts with water to generate nano titanium dioxide. The uniform distribution of the acid source in the composite material promotes the nano titanium dioxide to be uniformly distributed in the composite material and inhibits the size growth of the nano titanium dioxide, so that on the premise of ensuring the light transmittance of the polymethyl methacrylate, the composite material is endowed with ultraviolet absorption performance, and the toxicity possibly generated when an organic ultraviolet absorbent is used is avoided. The material can be used for biological optical materials such as artificial corneas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite materials, and more specifically, to a polymethyl methacrylate / nano titanium dioxide composite material and a preparation method and application thereof. Background Art

[0002] An artificial cornea is an artificial refractive device made of biomedical materials that is similar to a donor cornea. It is used to replace the diseased cornea to treat corneal diseases. Due to the lack of donor cornea sources and the low success rate of allogeneic corneal transplantation, donor corneas are far from meeting the needs of corneal disease treatment. Therefore, the development of materials suitable for the production of artificial corneas has great research significance and practical value.

[0003] Acrylic polymers (PHEMA, PMMA, etc.), polyvinyl alcohol (PVA), silicone gel and glass are used as the central lens column materials of artificial corneas because of their excellent transparency and light transmittance. Commonly used artificial cornea scaffold materials include inorganic materials, autologous biological materials and hydrogels. Among them, polymethyl methacrylate (PMMA) is a relatively ideal optical lens column material, which has the advantages of high light transmittance, good refractive index and easy processing. At present, artificial corneas based on PMMA include the most popular Boston artificial cornea, the Osteo-Odonto artificial cornea with a bone-tooth structure, and the MICOF artificial cornea developed and researched by the Moscow Eye Center.

[0004] As we all know, ultraviolet rays can cause eye damage, so as an artificial cornea material, it needs to have a high ultraviolet absorption rate, but PMMA's absorption rate of ultraviolet light is not high, and there is still a lot of room for improvement. Adding organic ultraviolet absorbers to polymer materials including PMMA to absorb ultraviolet rays, thereby improving the anti-ultraviolet aging performance of polymer materials or blocking ultraviolet transmission is a common method in industry. However, in a body fluid environment, since organic ultraviolet absorbers may dissolve from PMMA, there is a risk of poisoning human eye tissue. Nano-titanium dioxide is a biocompatible inorganic oxide and has good shielding and absorption properties for ultraviolet rays. Therefore, the use of nano-titanium dioxide as a polymer ultraviolet absorber has also attracted people's attention. Compared with organic ultraviolet absorbers, inorganic titanium dioxide nanoparticles are large in size and are not easily dissolved from PMMA. In addition, nano-titanium dioxide is one of the commonly used biomaterials and will not cause harm to the human body.

[0005] However, it is difficult to evenly disperse nano-titanium dioxide in polymers. Under high shear processing conditions such as screw extrusion, nano-titanium dioxide tends to agglomerate and increase in particle size. Large-sized nano-titanium dioxide not only reduces its UV absorption capacity, but also reduces the transparency of PMMA due to light scattering, making it unsuitable for use as a lens column material for artificial corneas.

[0006] Therefore, controlling the size of titanium dioxide and its uniform dispersion in PMMA is the key to obtaining high-performance PMMA / nano-titanium dioxide composites with UV absorption ability. Summary of the invention

[0007] In view of this, the main purpose of the present invention is to provide a polymethyl methacrylate / nano-titanium dioxide composite material with good dispersibility, low agglomeration, high ultraviolet absorption capacity and high safety.

[0008] In order to achieve the above technical objectives, the technical solution of the present invention is:

[0009] A polymethyl methacrylate / nano titanium dioxide composite material, the raw materials of the composite material comprising the following components in parts by weight: 800-1200 parts of methyl methacrylate, 10-1200 parts of a titanium source, 30-80 parts of an acid source, 2-15 parts of an initiator, and 1-5 parts of water;

[0010] Wherein, the acid source is methacrylic acid or acrylic acid.

[0011] Furthermore, the raw materials also include 20 to 40 parts of a cross-linking agent.

[0012] Furthermore, the titanium source is one or a combination of tetrabutyl titanate, tetraethyl titanate, tetrapropyl titanate, and titanium tetrachloride.

[0013] Further, the initiator is a photoinitiator or a thermal initiator;

[0014] The photoinitiator is benzoin, benzoin dimethyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, diphenyl acetone, a, a-dimethoxy-a-phenyl acetophenone, a, a-diethoxy acetophenone, α-hydroxyalkyl phenone, 2-hydroxyisobutyrophenone (D-1173), α-aminoalkyl phenone, aromatic acyl phosphine oxide, bisbenzoylphenyl phosphine oxide, benzophenone, 2,4-dihydroxybenzophenone, Michler's ketone, thiopropoxythioxanthone, isopropylthioxanthone, 2-hydroxy-2-methyl-1-phenylacetone , 1-hydroxycyclohexylphenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-dimethylamino-2-benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, methyl benzoylformate, at least one of IHT-PI4265, IHT-PI 1000, and IHT-PI 500; wherein IHT-PI4265, IHT-PI 1000, and IHT-PI 500 are trade names and can be purchased;

[0015] The thermal initiator is selected from at least one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, diisopropyl peroxydicarbonate, potassium persulfate, ammonium persulfate, 1-hydroxycyclohexyl phenyl ketone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, methyl benzoylformate, benzoin dimethyl ether, diphenyl acetone, α-aminoalkyl phenone, bisbenzoylphenylphosphine oxide, benzophenone and isopropylthioxanthone.

[0016] A second object of the present invention is to provide a method for preparing any of the above-mentioned composite materials, comprising the following steps:

[0017] (1) Weighing the raw materials in parts by mass;

[0018] (2) mixing an acid source, methyl methacrylate, a titanium source and an initiator into a uniform reaction solution;

[0019] (3) adding water to the reaction solution and stirring and ultrasonic treatment;

[0020] (4) After ultrasonic treatment, polymerization is carried out under ultraviolet light or elevated temperature conditions to obtain a polymethyl methacrylate / nano-titanium dioxide composite material.

[0021] Furthermore, in step (3), the stirring time is 20 to 30 minutes, the stirring speed is 200 to 400 rpm, the ultrasonic time is 8 to 20 minutes, and the ultrasonic intensity is 100 to 150W.

[0022] Furthermore, when the initiator in the raw material is a photoinitiator, in step (4), polymerization is carried out under ultraviolet light, wherein the wavelength of the ultraviolet light is 300 to 400 nm and the power of the ultraviolet light is 800 to 1000 mW / cm 2 The polymerization time under ultraviolet conditions is 15 to 30 minutes.

[0023] Furthermore, when the initiator in the raw materials is a thermal initiator, in step (4), the polymerization is carried out under heating conditions, wherein the temperature is first raised to 45-55°C, the polymerization reaction is carried out for 4-7 hours, the temperature is then raised to 100-110°C, the polymerization reaction is carried out for 1.5-3 hours, and the temperature is then lowered to room temperature.

[0024] The present invention also aims to provide the application of the composite material or the composite material prepared by the above-mentioned preparation method in biological and medical materials.

[0025] Furthermore, the biological and medical materials include artificial corneas, artificial cartilage tissues, drug carriers, antibacterial materials and biosensors.

[0026] The beneficial effects of the present invention are:

[0027] (1) The polymer formed by UV-curing or heat-curing of MMA, titanium source, acid source, initiator and water in the present invention has good biocompatibility, strong absorption rate of UV light, and can better avoid the harm of UV light to the eyes. It also has excellent mechanical properties and tensile strength greater than normal intraocular pressure (1.66KPa~2.80KPa), which can meet the use requirements of artificial cornea.

[0028] (2) Nano-TiO2 has become a material with good thermal stability and light corrosion resistance due to its high chemical stability, non-toxicity, high UV absorption rate and low cost. Introducing it into PMMA material can improve the UV absorption rate of artificial cornea and effectively maintain the excellent light transmittance of the optical center of artificial cornea. Its nano-size can ensure that it cannot migrate from the polymer molecular network into human tissue, thereby avoiding potential toxic side effects.

[0029] (3) The acid source plays a vital role in the preparation process of this material. The acid source molecules enter the molecular network of PMMA due to the polymerization reaction and can be evenly distributed in the molecular network of PMMA. These acid source molecules act as catalysts for the titanium source to generate nano-titanium dioxide. They will become the active centers of the reaction and prompt the nano-titanium dioxide to be evenly distributed in the molecular network of PMMA. They not only clear the surrounding titanium source small molecules, but also limit the size of nano-titanium dioxide, thereby forming nano-titanium dioxide with higher ultraviolet absorption capacity and preventing the migration and agglomeration of nano-titanium dioxide.

[0030] (4) The PMMA / nano-TiO2 composite material prepared by the present invention has a wide range of applications and can be applied to various biological and medical materials, such as artificial cartilage tissue, drug carriers, antibacterial materials and biosensors, etc.

[0031] (5) The preparation method of the present invention is simple, the conditions are mild, and it is convenient for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The experimental results of ultraviolet light absorption rate of PMMA / nano-TiO2 composite materials prepared in Example 1 (black curve), Comparative Examples 1 (red curve) and 2 (blue curve) are shown.

[0033] Figure 2 The experimental results of ultraviolet light absorption rate of PMMA / nano-TiO2 composite material prepared in Example 2 are shown.

[0034] Figure 3 The experimental results of ultraviolet light absorption rate of PMMA / nano-TiO2 composite material prepared in Example 3 are shown.

[0035] Figure 4 The experimental results of ultraviolet light absorption rate of PMMA / nano-TiO2 composite material prepared in Example 4 are shown.

[0036] Figure 5 These are the experimental results of the ultraviolet light absorption rate of the PMMA / nano-TiO2 composite material prepared in Example 5. DETAILED DESCRIPTION

[0037] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.

[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0039] Example 1

[0040] S1: Take the following raw materials by mass: 1 kg of methyl methacrylate, 15 g of 2-hydroxyisobutyrophenyl (D-1173), 3 g of ultrapure water, 50 g of methacrylic acid, and 10 g of tetrabutyl titanate. Stir the prepared raw material mixture evenly for 25 min at a stirring speed of 300 rpm, and then ultrasonicate for 10 min at an ultrasonic intensity of 120 W.

[0041] S2: Inject the mixed solution into the mold at a wavelength of 365nm and a power of 900mW / cm 2 The mixture was cured by ultraviolet light for 20 minutes to react, and the mixture changed from liquid to solid, thereby obtaining a PMMA / nano-TiO2 composite material, namely, sample 1.

[0042] The composite material (sample 1) prepared in this example was subjected to the following tests, and the results are shown in Table 1 below:

[0043] Table 1. Effects of different monomers on silicone hydrogel contact lenses

[0044]

[0045] Example 2

[0046] S1: Take by mass: 1 kg of methyl methacrylate, 15 g of 2-hydroxyisobutyrophenone (D-1173), 3 g of ultrapure water, 50 g of methacrylic acid, and 20 g of tetrabutyl titanate. Stir the prepared polymerization monomer mixture evenly for 25 minutes and then ultrasonicate for 10 minutes.

[0047] S2: The method is the same as in Example 1.

[0048] The composite material (sample 2) prepared in this example was subjected to the following tests, and the results are shown in Table 2 below:

[0049] Table 2. Effects of different monomers on silicone hydrogel contact lenses

[0050]

[0051] Embodiment 3:

[0052] S1: Take by mass: 1 kg of methyl methacrylate, 15 g of 2-hydroxyisobutyrophenone (D-1173), 3 g of ultrapure water, 50 g of methacrylic acid, and 30 g of tetrabutyl titanate. Stir the prepared polymerization monomer mixture evenly for 25 minutes and then ultrasonicate for 10 minutes.

[0053] S2: The preparation method is the same as that of Example 1.

[0054] The composite material (sample 3) prepared in this example was subjected to the following tests, and the results are shown in Table 3 below:

[0055] Table 3. Effects of different monomers on silicone hydrogel contact lenses

[0056]

[0057] Embodiment 4:

[0058] S1: Take by mass: 1kg of methyl methacrylate, 15g of 2-hydroxyisobutyrophenyl (D-1173), 3g of ultrapure water, 50g of methacrylic acid, 30g of crosslinking agent, and 40g of tetrabutyl titanate. Stir the prepared polymerization monomer mixture evenly for 25min and then ultrasonicate for 10min.

[0059] S2: The preparation method is the same as that of Example 1.

[0060] The composite material (sample 4) prepared in this example was subjected to the following tests, and the results are shown in Table 4 below:

[0061] Table 4. Effects of different monomers on silicone hydrogel contact lenses

[0062]

[0063] Embodiment 5:

[0064] S1: Take by mass: 1 kg of methyl methacrylate, 15 g of 2-hydroxyisobutyrophenone (D-1173), 3 g of ultrapure water, 50 g of methacrylic acid, 30 g of crosslinking agent, and 50 g of tetrabutyl titanate. Stir the prepared polymerization monomer mixture evenly for 25 min and then ultrasonicate for 10 min.

[0065] S2: The preparation method is the same as that of Example 1.

[0066] The composite material (sample 5) prepared in this example was subjected to the following tests, and the results are shown in Table 5 below:

[0067] Table 5. Effects of different monomers on silicone hydrogel contact lenses

[0068]

[0069] Embodiment 6:

[0070] S1: Take by mass: 0.8 kg of methyl methacrylate, 2 g of diisopropyl peroxydicarbonate, 2 g of ultrapure water, 30 g of methacrylic acid, and 10 g of tetrabutyl titanate. Stir the prepared polymerization monomer mixture evenly for 25 min and then ultrasonicate for 10 min.

[0071] S2: inject the mixed solution into a mold, heat it to 50 degrees to polymerize for 6 hours, heat it to 105 degrees to polymerize for 2 hours, and cool it to room temperature. The mixture changes from liquid to solid to obtain a PMMA / nano-TiO2 composite material, i.e., sample 6.

[0072] The composite material prepared in this example was subjected to the following tests, and the results are shown in Table 6 below:

[0073] Table 6. Effects of different monomers on silicone hydrogel contact lenses

[0074]

[0075] Embodiment 7:

[0076] S1: Take by mass: 1.2 kg of methyl methacrylate, 10 g of methyl benzoylformate, 4 g of ultrapure water, 70 g of acrylic acid, and 10 g of tetrapropyl titanate. Stir the prepared polymerization monomer mixture evenly for 25 min and then ultrasonicate for 10 min.

[0077] S2: Inject the mixed solution into the mold at a wavelength of 365nm and a power of 900mW / cm 2 The mixture was cured by ultraviolet light for 20 minutes to react, and the mixture changed from liquid to solid, thereby obtaining a PMMA / nano-TiO2 composite material, i.e., Sample 7.

[0078] The composite material prepared in this example was subjected to the following tests, and the results are shown in Table 7 below:

[0079] Table 7. Effects of different monomers on silicone hydrogel contact lenses

[0080]

[0081] Embodiment 8:

[0082] S1: Take by mass: 1 kg of methyl methacrylate, 3 g of diisopropyl peroxydicarbonate, 3 g of ultrapure water, 40 g of acrylic acid, and 10 g of titanium tetrachloride. Stir the prepared polymerization monomer mixture evenly for 25 min and then ultrasonicate for 10 min.

[0083] S2: inject the mixed solution into a mold, heat it to 50 degrees to polymerize for 6 hours, heat it to 105 degrees to polymerize for 2 hours, and cool it to room temperature. The mixture changes from liquid to solid to obtain a PMMA / nano-TiO2 composite material, namely, sample 8.

[0084] The composite material prepared in this example was subjected to the following tests, and the results are shown in Table 8 below:

[0085] Table 8. Effects of different monomers on silicone hydrogel contact lenses

[0086]

[0087] Embodiment 9:

[0088] S1: Take by mass: 1.2 kg of methyl methacrylate, 2 g of azobisisoheptanenitrile, 3 g of ultrapure water, 50 g of acrylic acid, and 30 g of tetraethyl titanate. Stir the prepared polymerization monomer mixture evenly for 30 min and then ultrasonicate for 15 min.

[0089] S2: inject the mixed solution into a mold, heat it to 55 degrees to polymerize for 5 hours, heat it to 105 degrees to polymerize for 2 hours, and cool it to room temperature. The mixture changes from liquid to solid to obtain a PMMA / nano-TiO2 composite material, namely, sample 9.

[0090] The composite material prepared in this example was subjected to the following tests, and the results are shown in Table 9 below:

[0091] Table 9. Effects of different monomers on silicone hydrogel contact lenses

[0092]

[0093] Comparative Example 1

[0094] The only difference between this embodiment and embodiment 1 is that no acid source, namely methacrylic acid, is added, but 0.01 M hydrochloric acid solution is used instead of ultrapure water and methacrylic acid.

[0095] The remaining steps and components remain unchanged.

[0096] A PMMA / nano-TiO2 composite material was prepared as comparative sample 1.

[0097] Comparative Example 2

[0098] The only difference between this embodiment and embodiment 1 is that no acid source, ie, methacrylic acid, is added.

[0099] The remaining steps and components remain unchanged.

[0100] A PMMA / nano-TiO2 composite material was prepared as comparative sample 2.

[0101] The samples obtained from Comparative Examples 1 and 2 were also subjected to performance tests and compared with Sample 1. The results are shown in Table 10 below:

[0102] Table 10. Effects of different monomers on silicone hydrogel contact lenses

[0103]

[0104] At the same time, the ultraviolet light absorption rate of the materials obtained in Examples 1-5 and Comparative Examples 1-2 was measured. The results are as follows: Figure 1-5 When inorganic acid is used or no acid source is added, the titanium dioxide particles will become larger and unevenly distributed in the hydrogel, and the titanium dioxide nanoparticles will easily precipitate from the monomer and even diffuse to the surface of the silicone hydrogel. The precipitated titanium dioxide will not only scatter light, but also form defects in the material, resulting in a decrease in light transmittance (see Figure 1 ), the elongation at break decreases. At the same time, the precipitation of nanoparticles will bring potential pathogenic risks.

[0105] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0106] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A polymethyl methacrylate / nano titanium dioxide composite material, characterized in that: The raw materials of the composite material include the following components in parts by weight: 800-1200 parts of methyl methacrylate, 10-50 parts of titanium source, 30-80 parts of acid source, 2-15 parts of initiator, and 1-5 parts of water; Wherein, the acid source is methacrylic acid or acrylic acid.

2. The polymethyl methacrylate / nano-titanium dioxide composite material according to claim 1, characterized in that: The raw materials also include 20 to 40 parts of a cross-linking agent.

3. The polymethyl methacrylate / nano-titanium dioxide composite material according to claim 1, characterized in that: The titanium source is one or a combination of tetrabutyl titanate, tetraethyl titanate, tetrapropyl titanate and titanium tetrachloride.

4. The polymethyl methacrylate / nano-titanium dioxide composite material according to claim 1, characterized in that: The initiator is a photoinitiator or a thermal initiator; The photoinitiator is benzoin, benzoin dimethyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, diphenyl acetone, a, a-dimethoxy-a-phenyl acetophenone, a, a-diethoxy acetophenone, α-hydroxyalkyl phenone, 2-hydroxyisobutyrophenone, α-aminoalkyl phenone, aromatic acyl phosphine oxide, bisbenzoylphenyl phosphine oxide, benzophenone, 2,4-dihydroxybenzophenone, Michler's ketone, thiopropoxythioxanthone, isopropylthioxanthone, 2-hydroxy-2-methyl-1-phenyl At least one of acetone, 1-hydroxycyclohexylphenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-dimethylamino-2-benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, and methyl benzoylformate; The thermal initiator is selected from at least one of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, diisopropyl peroxydicarbonate, potassium persulfate, ammonium persulfate, 1-hydroxycyclohexyl phenyl ketone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, methyl benzoylformate, benzoin dimethyl ether, diphenyl acetone, α-aminoalkyl phenone, bisbenzoylphenylphosphine oxide, benzophenone and isopropylthioxanthone.

5. The method for preparing the composite material according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Weighing the raw materials in parts by mass; (2) mixing an acid source, methyl methacrylate, a titanium source and an initiator into a uniform reaction solution; (3) adding water to the reaction solution and stirring and ultrasonic treatment; (4) After ultrasonic treatment, polymerization is carried out under ultraviolet light or elevated temperature conditions to obtain a polymethyl methacrylate / nano-titanium dioxide composite material.

6. Application of the composite material according to any one of claims 1 to 4 or the composite material prepared by the preparation method according to claim 5 in biological and medical materials.

7. The use according to claim 6, characterized in that: The biological and medical materials include artificial cornea, artificial cartilage tissue, drug carrier, antibacterial material and biosensor.