Sand prevention and water control polymer as well as preparation method and application thereof

The sand control and water control polymer, a copolymer of acrylamide, acryloyloxyethyltrimethylammonium chloride and methacryloyloxyethyldimethylbenzylammonium chloride, has solved the problems of sand production and high water content in oil fields, achieving integrated sand control and water control, reducing construction costs and improving operational efficiency.

CN118930728APending Publication Date: 2024-11-12CHINA OILFIELD SERVICES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411256615.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing technologies cannot effectively solve the problems of sand production and high water cut in oil fields at the same time, especially in sandstone reservoirs, where sand control and water control measures are costly and ineffective when implemented alone.

Method used

A copolymer of acrylamide, acryloyloxyethyltrimethylammonium chloride and methacryloyloxyethyldimethylbenzylammonium chloride is used as a sand control and water control polymer. Through electrostatic adsorption and associative bridging, sand control and water control are integrated.

Benefits of technology

It solves the problems of sand production and high water cut in loose sandstone reservoirs, has good sand control and water control capabilities, is low in cost, environmentally friendly, and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930728A_ABST
    Figure CN118930728A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of oilfield chemistry, and particularly relates to a sand-preventing and water-controlling polymer as well as a preparation method and application thereof. The sand prevention and water control polymer provided by the invention is a copolymer of acrylamide, acryloyloxyethyl trimethyl ammonium chloride and methacryloyloxyethyl dimethyl benzyl ammonium chloride. The sand-preventing and water-controlling polymer has excellent sand-preventing and water-controlling capability, has the advantages of good injectability, environment-friendly raw materials, low cost, large-scale production and application and the like, has a sand-preventing function and a water-controlling function, and effectively solves the problems of sand production and high water content of an oil well of a loose sandstone reservoir.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oilfield chemistry, and in particular relates to a sand control and water control polymer and a preparation method and application thereof. Background Art

[0002] At present, most of my country's oil fields are in the middle and late stages of development, and the water content of some oil fields has exceeded 90%. The problems of high water content and sand production in oil fields have become increasingly prominent. How to effectively control sand production and high water content is an important problem in production increase measures. Among them, sand production and high water content in sandstone reservoirs are the most serious. The rock cementation strength of this type of reservoir is weak, the cementation content is small, the distribution is uneven, and the geological age is late. It is more likely to cause sand production as the water content of the formation increases, the capillary force decreases, and the high shear flow rate destroys the formation skeleton structure; sand production in the formation will lead to a decrease in reservoir strength and an increase in heterogeneity, which will further increase the water content. The two have a reverse promotion effect, which has an adverse effect on oil field oil stability and water control.

[0003] my country's sandstone reservoirs are widely distributed and cover a large area, and their reserves occupy an important position. In order to meet the production needs of oil fields, the number of sand control and water control measures implemented separately has increased year by year, which not only makes oil and water well operations frequent, but also greatly increases costs. According to statistics, 48% of oil wells are prone to sand production after a single water plugging measure, and 50% of oil wells still have high water content after a single sand control measure. It can be seen that high water content and sand production will affect each other, and a means is urgently needed to achieve simultaneous sand control and water control.

[0004] The invention patent with publication number CN104861110A discloses a high permeability heavy oil reservoir anti-swelling and sand-inhibiting agent and its preparation method, which prepares an anti-swelling and sand-inhibiting agent suitable for high permeability heavy oil reservoirs, which is copolymerized by 10% to 35% acrylamide or methacrylamide, 5% to 25% 2-acrylamide-2-methylpropane sulfonate, 1% to 5% styrene or acrylonitrile, and 5% to 20% acryloyloxyethyl trimethyl ammonium chloride or trimethyl allyl ammonium chloride. The anti-swelling and sand-inhibiting agent is suitable for medium and high permeability heavy oil reservoirs at 70°C to 120°C, and has good effects in preventing clay expansion and inhibiting sand migration. It can not only inhibit reservoir clay expansion and inhibit formation sand dispersion and migration, but also effectively prevent fine sand and fine sand in the formation from flowing into the wellbore. However, its synthetic monomers are of many types, high cost, and easy to pollute the environment (styrene is highly toxic), which is not conducive to large-scale production and application.

[0005] The invention patent with publication number CN 103012667A discloses an oil well sand and water blocking agent, which is synthesized with acrylamide, sodium acrylate, and N,N-methylenebisacrylamide as raw materials. The sand and water blocking agent can be adsorbed on the surface of gravel and consolidate sand through self-cementation, and has good sand and water control effects and a long effective period. However, it has the disadvantages of both water blocking and oil blocking, and cannot achieve the function of "swelling when encountering water and shrinking when encountering oil"; in addition, due to the limited pumping time, injecting high-viscosity resin / gel solution into the sand-producing layer section is likely to lead to poor injectability in reservoirs with low permeability, and is not suitable for low permeability sand-producing layers.

[0006] Therefore, developing a system with sand prevention and water control functions that takes into account both sand prevention and water control functions and can simultaneously control sand production and high water content problems in one construction has gradually become an important trend and research direction for solving the problems of sand production and high water content. Summary of the invention

[0007] In view of the defects of the prior art, the present invention provides a sand control and water control polymer and a preparation method and application thereof.

[0008] Specifically, the sand control and water control polymer provided by the present invention is a copolymer of acrylamide, acryloyloxyethyltrimethylammonium chloride and methacryloyloxyethyldimethylbenzylammonium chloride.

[0009] In the above-mentioned sand control and water control polymer, the content of acrylamide is 10-16 parts by weight, the content of acryloyloxyethyl trimethyl ammonium chloride is 28-44 parts by weight, and the content of methacryloyloxyethyl dimethyl benzyl ammonium chloride is 6-12 parts by weight.

[0010] The above-mentioned sand control and water control polymer has, by weight, 10.5 to 16.1 parts of acrylamide, 28.5 to 43.9 parts of acryloyloxyethyl trimethyl ammonium chloride, and 6.1 to 11.6 parts of methacryloyloxyethyl dimethyl benzyl ammonium chloride.

[0011] On the other hand, the present invention also provides a method for preparing the above-mentioned sand control and water control polymer, comprising:

[0012] (1) dissolving acrylamide, acryloyloxyethyl trimethyl ammonium chloride and methacryloyloxyethyl dimethyl benzyl ammonium chloride in water according to a ratio;

[0013] (2) Adjust the pH to 6-7 and introduce inert gas to remove oxygen;

[0014] (3) After the temperature of the reaction system is lowered to ≤10°C, an initiator is added and the reaction is carried out;

[0015] (4) heating and raising the temperature, and continuing the reaction until the reaction is completed, thereby obtaining a sand control and water control polymer.

[0016] The method for preparing the sand control and water control polymer further comprises, after step (4): (5) vacuum freeze-drying and pulverizing the sand control and water control polymer.

[0017] In the above-mentioned method for preparing the sand control and water control polymer, the mass of the initiator is 0.1%-0.5% of the total mass of each monomer, wherein the initiator comprises sodium formaldehyde sulfoxylate and hydrogen peroxide in a weight ratio of 1:1-1:2.

[0018] In the above-mentioned method for preparing the sand control and water control polymer, the water is deionized water.

[0019] In the above-mentioned method for preparing the sand control and water control polymer, in step (3), the reaction temperature is 0-10° C. and the reaction time is 4-8 hours.

[0020] In the above-mentioned method for preparing the sand control and water control polymer, in step (4), the heating temperature is 40-60° C., and the duration of the continued reaction is 2-5 hours.

[0021] In another aspect, the present invention further provides use of the above-mentioned sand control and water control polymer or the sand control and water control polymer prepared by the above-mentioned preparation method in loose sandstone reservoirs.

[0022] Compared with the prior art, the sand control and water control polymer of the present invention has the following beneficial effects:

[0023] (1) The present invention uses polymer chains as chimeric carriers, introduces functional monomers with adsorption and associative bridging effects into the polymer chains, and utilizes the synergistic effect between the functional monomers to prepare a polymer with sand control and water control, thereby achieving integrated sand control and water control, and solving the problems of sand production and high water content in the formation;

[0024] (2) The sand-controlling and water-controlling polymer of the present invention has excellent sand-controlling and water-controlling capabilities, and has the advantages of good injectability, environmentally friendly raw materials, low cost, and large-scale production and application. It has both sand-controlling and water-controlling functions, and effectively solves the problems of sand production and high water content in oil wells in loose sandstone reservoirs. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the following detailed description of the preferred embodiment.The drawings are only for the purpose of illustrating the preferred embodiments and are not to be construed as limiting the invention.

[0026] Figure 1 This is the H-NMR spectrum of the sand control and water control polymer prepared in Example 1.

[0027] Figure 2 Graph for field application. DETAILED DESCRIPTION

[0028] In order to fully understand the purpose, features and effects of the present invention, the present invention is described in detail through the following specific embodiments. Except for the following contents, the process method of the present invention adopts conventional methods or devices in the art. Unless otherwise specified, the following terms have the meanings commonly understood by those skilled in the art.

[0029] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe a feature or characteristic, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0030] In view of the characteristics of sandstone reservoirs such as strong heterogeneity, high porosity and high permeability within the layer, and poor cementation of sand particles, and combined with the current scarce research on sand control and water control agents, the present invention uses polymer chains as chimeric carriers, introduces functional monomers with adsorption and associative bridging effects into them, and utilizes the synergistic effect between the functional monomers to prepare a sand control and water control polymer, thereby achieving integrated sand control and water control, and simultaneously solving the problems of sand production and high water content in the formation.

[0031] Specifically, in the first aspect, the sand control and water control polymer provided by the present invention is a copolymer of acrylamide, acryloyloxyethyltrimethylammonium chloride and methacryloyloxyethyldimethylbenzylammonium chloride.

[0032] In the sand control and water control polymer of the present invention, acryloyloxyethyl trimethyl ammonium chloride (DAC) is a cationic monomer, which can produce a strong electrostatic adsorption effect with quartz sand; methacryloyloxyethyl dimethyl benzyl ammonium chloride (DBC) is a hydrophobic monomer, which can make the polymer molecules adsorbed on the surface of quartz sand produce bridging association to achieve a better agglomeration effect of sand particles. The present invention obtains a polymer with the dual functions of sand control and water control by copolymerizing acryloyloxyethyl trimethyl ammonium chloride, methacryloyloxyethyl dimethyl benzyl ammonium chloride and acrylamide with the synergistic effect of the three monomers, realizing the integrated technology of sand control and water control, greatly reducing construction costs and improving operation effects.

[0033] In some preferred embodiments, the content of acrylamide is 10-16 parts by weight, the content of acryloyloxyethyl trimethyl ammonium chloride is 28-44 parts by weight, and the content of methacryloyloxyethyl dimethyl benzyl ammonium chloride is 6-12 parts by weight.

[0034] In practice, when too much acryloyloxyethyl trimethyl ammonium chloride is added, the polymerization reaction is incomplete and the monomer conversion rate is low; when too little is added, the cationic characteristics are not obvious and the adsorption effect on sand particles is poor. When too much methacryloyloxyethyl dimethyl benzyl ammonium chloride is added, the polymerization product is easy to cross-link, resulting in poor solubility; when too little is added, the associative bridging effect is not obvious, and the bundling and agglomeration effect on sand particles is weakened.

[0035] More preferably, in parts by weight, the content of acrylamide is 10.5 to 16.1 parts, the content of acryloyloxyethyl trimethyl ammonium chloride is 28.5 to 43.9 parts, and the content of methacryloyloxyethyl dimethyl benzyl ammonium chloride is 6.1 to 11.6 parts.

[0036] In a second aspect, the present invention also provides a method for preparing the above-mentioned sand control and water control polymer, comprising:

[0037] (1) dissolving acrylamide, acryloyloxyethyl trimethyl ammonium chloride and methacryloyloxyethyl dimethyl benzyl ammonium chloride in water according to a ratio;

[0038] (2) Adjust the pH to 6-7 and introduce inert gas to remove oxygen;

[0039] (3) After the temperature of the reaction system is lowered to ≤10°C, an initiator is added and the reaction is carried out;

[0040] (4) heating and raising the temperature, and continuing the reaction until the reaction is completed, thereby obtaining a sand control and water control polymer.

[0041] The sand control and water control polymer of the present invention adopts the existing aqueous solution free radical polymerization applicable to industrial large-scale production, and the exterior of the reaction kettle adopts a heat insulation method, which is conducive to directly scaling up indoor experiments for industrial production.

[0042] The ratios of acrylamide, acryloyloxyethyl trimethyl ammonium chloride and methacryloyloxyethyl dimethyl benzyl ammonium chloride involved in step (1) are the same as those in the sand control and water control polymer provided in the first aspect of the present invention, and the present invention will not repeat them here.

[0043] The chemical reactions involved are as follows:

[0044]

[0045] Among them, HP is hydrogen peroxide, SFS is sodium formaldehyde sulfoxylate, and X, Y, and Z are the values ​​of each monomer participating in the reaction in the chemical synthesis equation.

[0046] In some preferred embodiments, the method for preparing the sand control and water control polymer of the present invention further comprises step (5): vacuum freeze-drying and pulverizing the sand control and water control polymer.

[0047] In some preferred embodiments, the mass of the initiator used in the present invention is 0.1%-0.5% of the total mass of each monomer, wherein the initiator comprises sodium formaldehyde sulfoxylate and hydrogen peroxide in a weight ratio of 1:1-1:2.

[0048] The initiator used in the present invention is a redox system, which can generate free radicals at low temperature to initiate polymerization reaction, making it easier for the polymer product to form a high molecular weight product.

[0049] Deionized water has high purity and few impurities, making it easier for the polymerization reaction to form a high molecular weight product. Therefore, in some preferred embodiments, the water used in the present invention is deionized water.

[0050] Low temperature reaction slows down the generation of free radicals, so that the individual monomer molecules are orderly embedded together to form a high molecular polymer, and the product formed changes from a solution before the reaction to a gel after the reaction. In some preferred embodiments, the reaction temperature of step (3) is 0-10°C and the reaction time is 4-8 hours.

[0051] More preferably, the reaction temperature of step (3) is 5-10° C., and the reaction time is 6 hours.

[0052] In the polymerization reaction, heating can accelerate the reaction rate, so that the monomers that have not reacted under low temperature conditions are re-embedded in the polymer chain, increasing the molecular weight of the polymer and improving the monomer conversion rate. In some preferred embodiments, the heating temperature is 40-60°C, and the reaction time is 2-5 hours.

[0053] More preferably, the heating temperature in step (4) is 50° C. and the reaction time is 2 hours.

[0054] The preparation method of the sand-controlling and water-controlling polymer of the present invention starts from the principle of molecular structure design, and preferably selects the cationic monomer acryloxyethyl trimethyl ammonium chloride (DAC) which has low cost, good effect, is environmentally friendly and can be mass-produced and can produce strong electrostatic adsorption with quartz sand, and the hydrophobic monomer methacryloyloxyethyl dimethyl benzyl ammonium chloride (DBC) which can make the polymer molecules adsorbed on the surface of quartz sand produce bridging association to achieve better sand agglomeration effect. A sand-controlling and water-controlling polymer that can be used in loose sandstone reservoirs is prepared by copolymerizing the two with acrylamide. The polymer exhibits excellent sand-controlling and water-controlling capabilities, has good injectability, is environmentally friendly with raw materials, has low cost, can be mass-produced and applied, and has the advantages of both sand-controlling and water-controlling functions, and effectively solves the problems of sand production and high water content in oil wells in loose sandstone reservoirs.

[0055] Example

[0056] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions. The raw materials used in the following examples are all conventionally purchased.

[0057] Example 1

[0058] Acrylamide, acryloyloxyethyl trimethyl ammonium chloride, and methacryloyloxyethyl dimethyl benzyl ammonium chloride were added to deionized water according to the ratio, wherein the concentration of acryloyl was 12%, the concentration of acryloyloxyethyl trimethyl ammonium chloride was 34%, and the concentration of methacryloyloxyethyl dimethyl benzyl ammonium chloride was 6%. The pH of the above solution was adjusted to neutral with an aqueous NaOH solution, and then the mixed solution was transferred to a three-necked flask, and nitrogen was passed through to deoxygenate for 30 minutes, and then the temperature of the reaction system was lowered to below 10°C, and an initiator accounting for 0.2% of the total weight of the monomer was added to initiate polymerization (the mass ratio of sodium formaldehyde sulfoxylate and hydrogen peroxide was 1:1.2), and the system was kept at 0-10°C for 6 hours, and then the temperature was raised to 50°C for 2 hours. After the reaction was completed, the final product was taken out from the three-necked flask, vacuum freeze-dried at -50°C, and crushed to obtain the target product 1.

[0059] Example 2

[0060] Acrylamide, acryloyloxyethyl trimethyl ammonium chloride, and methacryloyloxyethyl dimethyl benzyl ammonium chloride were added to deionized water according to the ratio, wherein the concentration of acrylamide was 14%, the concentration of acryloyloxyethyl trimethyl ammonium chloride was 36%, and the concentration of methacryloyloxyethyl dimethyl benzyl ammonium chloride was 7%. The pH of the above solution was adjusted to neutral with an aqueous NaOH solution, and then the mixed solution was transferred to a three-necked flask, and nitrogen was passed through to deoxygenate for 30 minutes, and then the temperature of the reaction system was lowered to below 10°C, and an initiator accounting for 0.3% of the total weight of the monomer was added to initiate polymerization (the mass ratio of sodium formaldehyde sulfoxylate and hydrogen peroxide was 1:1.4), and the system was kept at 0-10°C for 6 hours, and then the temperature was raised to 50°C for 2 hours. After the reaction was completed, the final product was taken out from the three-necked flask, vacuum freeze-dried at -50°C, and crushed to obtain the target product 2.

[0061] Example 3

[0062] Acrylamide, acryloyloxyethyl trimethyl ammonium chloride, and methacryloyloxyethyl dimethyl benzyl ammonium chloride were added to deionized water according to the ratio, wherein the concentration of acrylamide was 16%, the concentration of acryloyloxyethyl trimethyl ammonium chloride was 38%, and the concentration of methacryloyloxyethyl dimethyl benzyl ammonium chloride was 8%. The pH of the above solution was adjusted to neutral with an aqueous NaOH solution, and then the mixed solution was transferred to a three-necked flask, and nitrogen was passed through to deoxygenate for 30 minutes, and then the temperature of the reaction system was lowered to below 10°C, and an initiator accounting for 0.4% of the total weight of the monomer was added to initiate polymerization (the mass ratio of sodium formaldehyde sulfoxylate and hydrogen peroxide was 1:1.6), and the system was kept at 0-10°C for 6 hours, and then the temperature was raised to 50°C for 2 hours. After the reaction was completed, the final product was taken out from the three-necked flask, vacuum freeze-dried at -50°C, and crushed to obtain the target product 3.

[0063] Comparative Example 1

[0064] Comparative Example 1 uses a cationic polymer CP-50 with a 50% cationicity produced by Shandong Noel Chemical Co., Ltd. The product is obtained through commercial purchase.

[0065] Comparative Example 2

[0066] Comparative Example 2 uses the sand control and water control agent MEP produced by the French company Essen, which is obtained through commercial purchase.

[0067] Comparative Example 3

[0068] Comparative Example 3 uses a copolymerization product of acrylamide and methacryloyloxyethyl dimethylbenzyl ammonium chloride in a molar ratio of 94:6, and other polymerization reaction conditions are the same as those in Example.

[0069] Performance Testing

[0070] To further illustrate the product effect, the product performance of the present invention will be evaluated in conjunction with the examples below.

[0071] 1. Chemical structure characterization

[0072] The nuclear magnetic resonance spectroscopy test of Example 1 was performed. Figure 1 As shown, 7.5ppm is the absorption peak of the benzene ring skeleton; 4.7ppm is the absorption peak of heavy water; 3.9 / 3.4ppm is the absorption peak of the methylene group on the DAC side chain; 3.2ppm is the absorption peak of the quaternary ammonium group; 2.1ppm and 1.6, 1.2ppm are the absorption peaks of the methine, methylene and methyl groups on the polymer main chain. It can be seen that DAC and DBC are successfully grafted onto the polymer backbone, and the final product is the target copolymer.

[0073] 2. Evaluation of sand control effect

[0074] Experimental steps: By modifying and improving the existing technical requirements for sand inhibitors (Q / SH 1020 2377-2020), it can more effectively distinguish and screen the performance of sand inhibitors at 100mL / min. The experimental device and method refer to "Q / SH 1020 2377-2020". The sand filling pipe filled with 20-40 mesh quartz sand and 210-300 mesh kaolin in a mass ratio of 21.2:1.0 is connected to the displacement device. When ordinary single-layer 150-mesh screens are set at both ends of the sand pipe, saturated mineral water 2.0PV is injected at 1mL / min, and then 2.0PV polymer solution is injected in reverse, and sealed and aged for 12h. The driving pump speed is set to 100mL / min, simulate water displacement for 50min, and collect the discharged liquid. Filter all the liquid through quantitative medium-speed filter paper under stirring, transfer the filter paper and the filtrate into a beaker, put it into an oven at (105±2)℃ and dry it for 2 hours, then weigh it and calculate the amount of sand.

[0075] Experimental conditions: The concentration of sand control and water control polymer is 0.5%, the temperature is 65°C, the salt ion concentration of simulated water used in the experiment is 15000 mg / L, and the saturated volume of the functional polymer solution is 2.0 PV.

[0076] Table 1 Experimental results of sand control ability of sand control and water control polymer

[0077] Sand control and water control polymer Sand output μ(g / L) Example 1 0.0321 Example 2 0.0318 Example 3 0.0326 Comparative Example 1 0.0443 Comparative Example 2 0.0368 Comparative Example 3 0.0415

[0078] The experimental results show that the sand production of the sand-controlling and water-controlling polymer prepared by the present invention is μ<<0.05 g / L, which indicates that the sand-controlling and water-controlling polymer has good sand-controlling performance.

[0079] 3. Evaluation of water control effect

[0080] Experimental steps: The water-oil resistance ratio (NFRR) is the main indicator for measuring water control performance. This parameter can intuitively analyze the water-blocking but not oil-blocking effect of the water control agent. Fill two sand tubes with the same permeability (1000mD) and record them as S1 and S2. Saturate S1 and S2 with simulated water and crude oil respectively and record the permeabilities Kw and Ko when the pressure is stable. Then, reversely inject 0.5PV of functional polymer solution into S1 and S2 respectively and seal and age for 12h. Then, forwardly inject simulated water and crude oil into S1 and S2 respectively and record the permeabilities Kw' and Ko' when the pressure is stable. The water-oil resistance ratio (NFRR) is calculated as follows:

[0081]

[0082]

[0083]

[0084] Where: NFRR-standard fluid resistance ratio; RRF w -Residual resistance factor of water phase; RRF o -Oil phase residual resistance coefficient; k w - water permeability before plugging; k w‘ - water phase permeability after plugging; k o -Oil phase permeability before plugging; k o’ -Oil phase permeability after plugging.

[0085] Experimental conditions: The concentration of the sand control and water control polymer is 0.5%, the temperature is 65°C, the salt ion concentration of the simulated water used in the experiment is 15000 mg / L, the saturated volume of the sand control and water control polymer solution is 0.5 PV, and the crude oil viscosity is 540 mPa·s.

[0086] Table 2 Experimental results of water control ability of sand control and water control polymer

[0087] Sand control and water control polymer NFRR Example 1 5.13 Example 2 4.99 Example 3 5.04 Comparative Example 1 2.21 Comparative Example 2 2.90 Comparative Example 3 2.73

[0088] The experimental results show that the water-oil resistance ratio NFRR of the sand-controlling and water-controlling polymer prepared by the present invention is greater than 4.9, indicating that the sand-controlling and water-controlling polymer has good water-controlling performance.

[0089] 4. On-site application effect evaluation

[0090] The casing program of Well A is 13-3 / 8"×194.22m+9-5 / 8"×1699.40m. The well is a development horizontal well. The well completion method is open hole completion. The sand control method is 5-1 / 2" high-quality screen + gravel packing (133μm). The sand control string is 1691.22m-2077.29m, a total of 386m. The pump hanging position is 1098.96m, the well inclination is 34.15°, the production layer is NmⅡ 3D-1244 sand body, and ordinary electric pumps are put into production.

[0091] The average porosity of the reservoir section is 30.92%, the porosity distribution is relatively uniform, the average permeability is 641.93mD, the reservoir physical properties are good, the mud content is about 14.54%, and the oil layer thickness is 327.5m. Before the operation, the production was 30Hz, and the daily liquid production was 237m 3 , daily oil production 20.6m 3 , containing 91% water and about 0.02% sand. 225m3 of sand control and water control polymer working fluid with a mass concentration of 0.5% is being squeezed out. 3 , geothermal water replacement 25m 3 After the measures were taken, the pump frequency was gradually increased from 30Hz to 40Hz. The current daily liquid production is 430m3. 3 , daily oil production 51m 3 , water content 88.2%, water content decreased by 2.8% and no sand was found ( Figure 2), which plays a good role in preventing sand and controlling water and releasing production capacity.

[0092] The present invention has been disclosed above with preferred embodiments, but those skilled in the art should understand that these embodiments are only used to describe the present invention and should not be understood as limiting the scope of the present invention. It should be noted that all changes and substitutions equivalent to these embodiments should be deemed to be included in the scope of the claims of the present invention. Therefore, the scope of protection of the present invention should be based on the scope defined in the claims.

Claims

1. A sand control and water control polymer, characterized in that: The sand control and water control polymer is a copolymer of acrylamide, acryloyloxyethyl trimethyl ammonium chloride and methacryloyloxyethyl dimethyl benzyl ammonium chloride.

2. The sand control and water control polymer according to claim 1, characterized in that: In parts by weight, the content of acrylamide is 10-16 parts, the content of acryloyloxyethyl trimethyl ammonium chloride is 28-44 parts, and the content of methacryloyloxyethyl dimethyl benzyl ammonium chloride is 6-12 parts.

3. The sand control and water control polymer according to claim 1, characterized in that: In parts by weight, the content of acrylamide is 10.5 to 16.1 parts, the content of acryloyloxyethyl trimethyl ammonium chloride is 28.5 to 43.9 parts, and the content of methacryloyloxyethyl dimethyl benzyl ammonium chloride is 6.1 to 11.6 parts.

4. The method for preparing the sand control and water control polymer according to any one of claims 1 to 3, characterized in that: include: (1) dissolving acrylamide, acryloyloxyethyl trimethyl ammonium chloride and methacryloyloxyethyl dimethyl benzyl ammonium chloride in water according to a ratio; (2) Adjust the pH to 6-7 and introduce inert gas to remove oxygen; (3) After the temperature of the reaction system is lowered to ≤10°C, an initiator is added and the reaction is carried out; (4) heating and raising the temperature, and continuing the reaction until the reaction is completed, thereby obtaining a sand control and water control polymer.

5. The method for preparing the sand control and water control polymer according to claim 4, characterized in that: After step (4), the method further includes: (5) vacuum freeze-drying and crushing the sand control and water control polymer.

6. The method for preparing a sand control and water control polymer according to claim 4, characterized in that: The mass of the initiator is 0.1%-0.5% of the total mass of each monomer, wherein the initiator comprises sodium formaldehyde sulfoxylate and hydrogen peroxide in a weight ratio of 1:1-1:

2.

7. The method for preparing a sand control and water control polymer according to claim 4, characterized in that: The water is deionized water.

8. The method for preparing a sand control and water control polymer according to claim 4, characterized in that: In step (3), the reaction temperature is 0-10°C and the reaction time is 4-8 hours.

9. The method for preparing a sand control and water control polymer according to claim 4, characterized in that: In step (4), the heating temperature is 40-60° C., and the reaction time is 2-5 hours.

10. Use of the sand control and water control polymer according to any one of claims 1 to 3 or the sand control and water control polymer prepared by the preparation method according to any one of claims 4 to 9 in loose sandstone reservoirs.