Diaphragm additive, diaphragm slurry, secondary battery diaphragm and battery

By using fibrous separator additives in lithium-ion battery separator, the thermal runaway problem of the battery under extreme conditions is solved, the heat resistance of the separator and the electrolyte wetting ability are improved, the service life of the battery is extended, and the circulation performance is improved. Energy density.

CN118930749AInactive Publication Date: 2024-11-12SHENZHEN HAODYNE TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411419057.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Lithium-ion batteries are prone to thermal runaway under extreme conditions, causing the membrane to shrink or melt, which in turn causes a short circuit of the positive and negative electrodes. The existing ceramic/polymer composite separator has a low heat resistance temperature and high density, which affects the safety of the battery and reliability.

Method used

Fibrous diaphragm additives, including vinyl, heterocyclic and acrylate structural units, form a three-dimensional network structure through cross-linking, improve mechanical strength and dimensional stability, and adjust the mass ratio and aspect ratio of the structural units. Optimize the thermal stability and electrolyte wetting properties of the diaphragm.

Benefits of technology

It improves the heat resistance of the diaphragm and the electrolyte wetting property, avoids the risk of deformation and short circuit of the diaphragm at high temperatures, extends the service life of the battery, and improves the cycling performance and energy density of the battery.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of battery materials, in particular to a diaphragm additive, diaphragm slurry, a secondary battery diaphragm and a battery, the diaphragm additive comprises a polymer, and the polymer comprises a vinyl structural unit, a heterocyclic structural unit, an acrylate structural unit and a crosslinking structural unit; the mass ratio of the vinyl structural unit to the heterocyclic structural unit to the acrylate structural unit to the crosslinking structural unit is (60-85): (5-20): (5-15): (1-15); the diaphragm additive is of a fibrous structure, and the length-diameter ratio of the diaphragm additive is 5-20. The high-Tg fibrous diaphragm additive disclosed by the invention can keep the structural stability in a high-temperature environment, and deformation or failure of a diaphragm caused by thermal shrinkage is avoided, so that the safety and reliability of the diaphragm in the high-temperature environment are improved; and the wettability of the diaphragm on electrolyte is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a diaphragm additive, a diaphragm slurry, a secondary battery diaphragm and a battery. Background Art

[0002] Lithium-ion batteries (LIBs) are a type of portable energy storage device that has been widely used in consumer electronics, electric vehicles, and energy storage systems. Lithium-ion batteries are mainly composed of a positive electrode, a negative electrode, a separator, an electrolyte, and a battery casing. During the charging process, an external voltage is applied across the battery, and lithium ions (Li+) are deintercalated from the positive electrode material, enter the electrolyte, and migrate to the negative electrode through the separator, where they combine with electrons and embed into the negative electrode material. During discharge, the process is reversed, and lithium ions migrate from the negative electrode to the positive electrode.

[0003] However, lithium-ion batteries are prone to thermal runaway under extreme conditions (such as overcharging or puncture), causing the battery to burn or even explode. This is mainly due to the increase in temperature inside the battery, which causes the separator to shrink or melt, resulting in direct contact between the positive and negative electrodes and a short circuit, which in turn triggers a series of chain reactions. Existing lithium-ion battery separators are mainly composed of polyolefin porous membranes. The melting point of this type of material is lower than 200°C, and it is easy to deform at high temperatures and lose its isolation function.

[0004] In recent years, in order to improve the energy density of lithium-ion batteries, the compaction density of positive and negative electrode materials has been continuously increased, which has aggravated the expansion problem of the electrode during the charge and discharge cycle of the battery to a certain extent, causing the battery to deform, affecting its safety and reliability. In addition, as the battery capacity increases, the size and weight of the battery also increase, which brings challenges to the production and packaging of the battery, especially when the internal structure of the battery cell is loose and the mechanical strength is insufficient, which may cause the battery cell to deform or even fail to assemble normally.

[0005] In order to solve these problems, ceramic / polymer composite diaphragms made by coating boehmite (ALOOH) ceramic particles on the surface of the diaphragm substrate are now available on the market. Boehmite has good heat resistance and flame retardancy, and can prevent thermal shrinkage of the diaphragm to a certain extent, thereby reducing the risk of short circuit between the positive and negative electrodes. However, the use of boehmite ceramic particles also has some shortcomings, such as its low heat resistance temperature (about 130°C), high density, which leads to an increase in the overall mass of the battery, and the electrolyte wettability has reached its limit, which cannot further improve the performance of the battery cell. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a diaphragm additive, a diaphragm slurry, a secondary battery diaphragm and a battery.

[0007] In the first aspect, a membrane additive comprises a polymer, wherein the polymer comprises a main structural unit, a first functional structural unit, a second functional structural unit and a cross-linking structural unit; the polymer comprises a vinyl structural unit, a heterocyclic structural unit, an acrylate structural unit and a cross-linking structural unit; the mass ratio of the vinyl structural unit, the heterocyclic structural unit, the acrylate structural unit and the cross-linking structural unit is (60~85): (5~20): (5~15): (1~15); the membrane additive is a fibrous structure, and the aspect ratio of the membrane additive is 5~20.

[0008] In the present invention, the vinyl structural units are used to provide basic mechanical strength and chemical stability, the aromatic ring structural units and the heterocyclic structural units have the functions of improving thermal stability and chemical resistance, the acrylate structural units have good electrolyte affinity, can improve the electrolyte wettability of the diaphragm, and help the penetration and retention of the electrolyte, and the cross-linked structural units enhance the mechanical strength and dimensional stability of the diaphragm by forming a three-dimensional network structure.

[0009] As is well known in the art, the above-mentioned vinyl structural units are obtained by polymerizing monomers containing vinyl functional groups. Similarly, the propenyl structural units are obtained by polymerizing monomers containing propenyl functional groups, the acrylate structural units are obtained by polymerizing monomers containing acrylate functional groups, the heterocyclic structural units are obtained by polymerizing monomers containing heterocyclic rings, and the acrylate structural units are obtained by polymerizing monomers containing acrylate functional groups. Similarly, in the polymer, the mass ratio of the vinyl structural units, the heterocyclic structural units, the acrylate structural units and the cross-linking structural units is the ratio of the added amounts of the monomers containing vinyl functional groups, the propenyl functional groups, the aromatic ring-containing monomers, the heterocyclic ring-containing monomers, the acrylate functional group-containing monomers and the cross-linking monomers used in the preparation of the polymer.

[0010] The fibrous diaphragm additives do not have a clear directionality when interweaving, and heat is generally transferred along the fibers. The non-directional interweaving prevents heat from being transferred quickly. In addition, when the fibrous diaphragm additives are in contact with the hot surface, they are rarely in vertical contact, which makes it difficult for heat to be transferred to the diaphragm additives. Moreover, the contact points of the fibers can reach 80%, further increasing the thermal resistance when heat is transferred. The fibrous diaphragm additives themselves are opaque, and heat rays cannot be transferred in the fibrous diaphragm additives. In addition, the surface area of ​​the fibrous diaphragm additives is small, and the radiation received is also small, so that heat radiation is basically not transferred on the fibers. When the fibrous diaphragm additives are applied to the diaphragm, the energy resistance of the diaphragm is improved, and the thermal shrinkage performance of the diaphragm is improved.

[0011] The ratio of the length to the diameter (i.e., the aspect ratio) of the membrane additive is between 5 and 20 by adjusting the mass ratio of the heterocyclic structural unit and the acrylate structural unit. Preferably, the length of the membrane additive is 500-2500 nm, and the diameter of the membrane additive is 50-100 nm.

[0012] Specifically, the aspect ratio of the fibrous structure of the separator additive can be 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, etc., as long as the aspect ratio of the fibrous structure of the separator additive is in the range of 5 to 20. When the aspect ratio of the separator additive is less than 5, the heat resistance of the separator additive is poor; when the aspect ratio of the separator additive is greater than 20, the wettability of the separator additive is poor.

[0013] Preferably, the glass transition temperature of the polymer is ≥150° C., and the swelling degree of the polymer in the electrolyte is 20% to 50%.

[0014] In the present invention, the glass transition temperature of the polymer may be 150°C, 160°C, 170°C, 180°C, 190°C or 200°C, etc.

[0015] The swelling degree of the polymer in the electrolyte can be 20%, 30%, 40% or 50%, etc.

[0016] In the present invention, the high Tg separator additive can maintain the stability of its structure under high temperature conditions and is not easily deformed or softened. When applied to the separator, the heat resistance of the separator can be improved. During high-temperature charging or use, the separator will not shrink or melt due to the increase in temperature, thereby avoiding the risk of short circuit.

[0017] And the swelling degree in the present invention means that the diaphragm can absorb a certain amount of electrolyte in the electrolyte but will not expand excessively. This helps to improve the uniform distribution of the electrolyte in the diaphragm, thereby improving the wettability of the electrolyte and the ion conductivity. The appropriate swelling degree can also ensure the stability of the diaphragm in the electrolyte and avoid the degradation of mechanical properties caused by excessive swelling; this allows the diaphragm to maintain a good contact area in the electrolyte without losing its structural integrity due to excessive expansion. If the swelling degree of the diaphragm additive with a fibrous structure is greater than 50%, it will cause the air permeability time of the diaphragm to be prolonged after being immersed in the electrolyte. If the swelling degree of the diaphragm additive with a fibrous structure is less than 20%, it will affect the electrolyte wettability of the diaphragm.

[0018] Preferably, the vinyl structural unit is selected from one or more of a styrene structural unit, a vinyl pyrrolidone structural unit and a vinyl toluene structural unit.

[0019] The acrylic structural unit is selected from one or more of a methyl acrylate structural unit, an ethyl acrylate structural unit, a butyl acrylate structural unit, and an isooctyl acrylate structural unit.

[0020] The heterocyclic structural unit is selected from one or more of an N-phenylmaleimide structural unit, an isobornyl acrylate structural unit, an isobornyl methacrylate structural unit, a methyl methacrylate structural unit, and a cycloethyl methacrylate structural unit.

[0021] Preferably, the acrylic structural unit is selected from one or more of ethyl acrylate structural unit, butyl acrylate structural unit, isooctyl acrylate structural unit, hydroxypropyl acrylate structural unit and hydroxybutyl acrylate structural unit.

[0022] Preferably, the cross-linking structural unit is selected from one or more of a polyethylene glycol diacrylate structural unit, a divinylbenzene structural unit, and a trimethylolpropane triacrylate structural unit.

[0023] In the present invention, the trimethylolpropane triacrylate structural unit has three reaction sites and can form a highly cross-linked network structure, the divinylbenzene structural unit has high thermal stability and chemical stability, and the polyethylene glycol diacrylate structural unit has good dimensional stability.

[0024] The present invention also provides a method for preparing the above-mentioned membrane additive, and the specific steps are as follows: (1) Using methanol and water as solvents, wherein the weight ratio of methanol to water is 7:3, the first functional structural unit, the second functional structural unit and 1 / 2 cross-linking structural unit, and the reversible addition-fragmentation chain transfer agent 3-(benzylthiocarbonylthio)propionic acid are added into a reaction vessel, and azobisisobutyronitrile is added, and the mixture is heated to 70° C. under nitrogen protection and kept at a constant temperature for 8 hours for reaction.

[0025] (2) The main monomer and the remaining 1 / 2 cross-linking structural unit are added to the container of step (1), and azobisisobutyronitrile is added. Under nitrogen protection, the mixture is heated to 70° C. and maintained at a constant temperature for 8 hours to perform a polymerization reaction to prepare a diaphragm additive.

[0026] The present invention provides a diaphragm slurry prepared by using the diaphragm additive of the first aspect, ceramic particles, a ceramic binder, and a dispersant, with a mass ratio of (10-80): (20-90): (5-8): (0.5-2).

[0027] Among them, the ceramic particles are selected from one or more of alumina and boehmite; the ceramic adhesive is selected from SWA610 produced by Haodian, and the dispersant is selected from one or more of CMC and sodium polyacrylate.

[0028] In a third aspect, the present invention provides a secondary battery separator, comprising the separator slurry according to the second aspect.

[0029] In a fourth aspect, the present invention provides a battery comprising the secondary battery separator according to the third aspect.

[0030] Compared with the prior art, the present invention has the following beneficial effects: The high-Tg fibrous diaphragm additive of the present invention can maintain the stability of its structure in a high-temperature environment, avoid deformation or failure of the diaphragm due to thermal shrinkage, thereby improving the safety and reliability of the diaphragm in a high-temperature environment; improve the wettability of the diaphragm to the electrolyte, so that the electrolyte can be distributed in the diaphragm more quickly and evenly, and improve the wettability and ion conductivity of the electrolyte; by reducing the internal resistance of the diaphragm, the energy efficiency of the battery is improved, the energy loss is reduced, and the output power and energy density of the battery are improved; the use of the diaphragm additive significantly improves the cycle performance of the battery, so that the battery can still maintain a high capacity after multiple charges and discharges, thereby extending the service life of the battery. DETAILED DESCRIPTION

[0031] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the protection scope of the present invention.

[0032] Example 1

[0033] This embodiment provides a method for preparing a membrane additive, and the specific steps are as follows: Using methanol and water as solvents, wherein the weight ratio of methanol to water is 7:3, 10 parts of isobornyl methacrylate, 5 parts of isooctyl acrylate and 1 / 2 cross-linking structural units, a reversible addition-fragmentation chain transfer agent 3-(benzylthiocarbonylthio)propionic acid are added to a reaction vessel, azobisisobutyronitrile is added, and the mixture is heated to 70°C under nitrogen protection and kept at a constant temperature for 8 hours to react.

[0034] (2) 80 parts of styrene and 2.5 parts of ethylene glycol diacrylate were added to the container of step (1), and azobisisobutyronitrile was added. The mixture was heated to 70° C. and maintained at a constant temperature for 8 hours under nitrogen protection to carry out polymerization reaction, thereby preparing a diaphragm additive.

[0035] This embodiment also provides a diaphragm slurry, which is prepared by selecting the above-mentioned diaphragm additive, boehmite, SWA610, and CMC, and the mass ratio thereof is 50:50:6:1.

[0036] Example 2

[0037] Most of the steps in Example 2 are the same as those in Example 1, except that the ratio of styrene:isobornyl methacrylate:isooctyl acrylate:ethylene glycol diacrylate is 75:10:5:10.

[0038] This embodiment also provides a diaphragm slurry, which is prepared by selecting the above-mentioned diaphragm additive, boehmite, SWA610, and CMC, and the mass ratio thereof is 50:50:6:1.

[0039] Example 3

[0040] Most of the steps of Example 3 are the same as those of Example 1, except that the ratio of styrene:isobornyl methacrylate:isooctyl acrylate:ethylene glycol diacrylate is 70:10:5:15.

[0041] This embodiment also provides a diaphragm slurry, which is prepared by selecting the above-mentioned diaphragm additive, boehmite, SWA610, and CMC, and the mass ratio thereof is 50:50:6:1.

[0042] Example 4

[0043] Most of the steps of Example 4 are the same as those of Example 1, except that the ratio of styrene:isobornyl methacrylate:isooctyl acrylate:ethylene glycol diacrylate is 80:5:10:5.

[0044] This embodiment also provides a diaphragm slurry, which is prepared by selecting the above-mentioned diaphragm additive, boehmite, SWA610, and CMC, and the mass ratio thereof is 50:50:6:1.

[0045] Example 5

[0046] Most of the steps of Example 5 are the same as those of Example 1, except that the ratio of styrene:isobornyl methacrylate:isooctyl acrylate:ethylene glycol diacrylate is 80:10:5:5.

[0047] This embodiment also provides a diaphragm slurry, which is prepared by selecting the above-mentioned diaphragm additive, boehmite, SWA610, and CMC, and the mass ratio thereof is 30:70:6:1.

[0048] Example 6

[0049] Most of the steps of Example 6 are the same as those of Example 1, except that the ratio of styrene:isobornyl methacrylate:isooctyl acrylate:ethylene glycol diacrylate is 80:10:5:5.

[0050] This embodiment also provides a diaphragm slurry, which is prepared by selecting the above-mentioned diaphragm additive, boehmite, SWA610, and CMC, and the mass ratio thereof is 70:30:6:1.

[0051] Comparative Example 1 The diaphragm slurry of this comparative example is prepared by using boehmite, SWA610 and CMC, and the mass ratio thereof is 100:6:1.

[0052] Comparative Example 2 Compared with Example 1, an emulsifier, sodium dodecylbenzene sulfonate, is introduced to prepare a spherical diaphragm additive through emulsion polymerization.

[0053] Comparative Example 3 (1) Styrene: isobornyl methacrylate: isooctyl acrylate: ethylene glycol diacrylate = 85:10:5:0; (2) This embodiment also provides a diaphragm slurry, which is prepared by using the above-mentioned diaphragm additive, boehmite, SWA610, and CMC, and the mass ratio thereof is 50:50:6:1.

[0054] Comparative Example 4 (1) Styrene: isobornyl methacrylate: isooctyl acrylate: ethylene glycol diacrylate = 65:10:5:20; (2) This embodiment also provides a diaphragm slurry, which is prepared by using the above-mentioned diaphragm additive, boehmite, SWA610, and CMC, and the mass ratio thereof is 50:50:6:1.

[0055] The glass transition temperature of the membrane additives of Examples 1 to 6 and Comparative Examples 1 to 4 was tested using differential scanning calorimetry.

[0056] The membrane additives of Examples 1 to 6 and Comparative Examples 1 to 4 were tested for swelling in the electrolyte.

[0057] The separator slurries of Examples 1 to 6 and Comparative Examples 1 to 4 were coated on a 7 μm base film, coated on both sides with a thickness of 2 μm each, and rolled up to obtain a secondary battery separator.

[0058] The thickness of the diaphragms of Examples 1 to 6 and Comparative Examples 1 to 4 was tested using a micrometer.

[0059] The surface density test was performed on the separators of Examples 1 to 6 and Comparative Examples 1 to 4.

[0060] The test method for the surface density of the diaphragm is: cut the diaphragm into several discs of the same size and known area, weigh them, and the surface density = W / S, where W is the average weight of the diaphragm discs and S is the area of ​​the discs.

[0061] The electrolyte wettability test was performed on the separators of Examples 1 to 6 and Comparative Examples 1 to 4.

[0062] The test method of electrolyte wettability is as follows: the diaphragm prepared by the scheme of the present invention is cut into a size of 5×100 mm, 0.1 μL of lithium salt electrolyte is dropped, and the droplet diffusion length is tested.

[0063] The air permeability test was performed on the diaphragms of Examples 1 to 6 and Comparative Examples 1 to 4. The test results are shown in Table 1.

[0064] The test method for the air permeability time is: using a Gurley air permeability instrument for testing.

[0065] The heat shrinkage resistance test was performed on the separators of Examples 1 to 6 and Comparative Examples 1 to 4. The test results are shown in Table 1.

[0066] The test method for heat shrinkage resistance is: cut the diaphragm prepared by the scheme of the present invention into a specification of 100×100 mm, place it between two A4 papers, place it on an iron plate, transfer it to a 130°C oven and bake it for 1 hour, and test the change rate of the longitudinal width (MD) and the transverse width (TD) before and after.

[0067] The battery preparation method is as follows: the negative electrode sheet, the positive electrode sheet and the separator are assembled into a battery.

[0068] The battery performance of Examples 1-6 and Comparative Examples 1-4 was tested, and the test results are shown in Table 2.

[0069] The test method is as follows: (1) The test method of DCIR test is: ① Test temperature: 25℃; ② SOC: 0, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 100%; ③ DCIR test method: 3C discharge for 30s.

[0070] (2) High temperature storage performance: After fully charged, place the battery in an oven at 85°C for 8 hours, take it out and test the capacity. Capacity retention rate (%) = (discharge capacity after high temperature storage / discharge capacity before storage) × 100%.

[0071] (3) Cycle performance test: The battery is charged at 25°C at a constant current of 6000mA (2C) to 4.5V, then charged at a constant voltage with a cut-off current value of 150mA, and then discharged at a constant current of 3000mA to 3V. This is considered one cycle. After repeating this process 500 times, the capacity retention rate after 500 cycles (%) is calculated as (discharge capacity after 500 cycles / initial discharge capacity) × 100%.

[0072] Table 1 Tg ℃ Diaphragm thickness μm <![CDATA[Grammage g / m 2 > Infiltration mm Diaphragm ventilation time s / 100ml Thermal shrinkage%150℃ / 1h Example 1 158 11.1 4.17 41 174.5 2.5 Example 2 163 11.2 4.10 38 172.4 2.3 Example 3 169 11.1 4.22 35 175.5 1.8 Example 4 153 10.9 4.15 46 191.5 2.9 Example 5 158 10.9 4.98 34 184.5 2.8 Example 6 158 11.0 3.73 48 183.2 2.9 Comparative Example 1 / 11.0 5.80 25 198.3 8.9 Comparative Example 2 154 11.2 4.18 32 195.6 7.5 Comparative Example 3 102 10.9 4.21 38 198.6 9.3 Comparative Example 4 Reunion / / / / / Table 2 DCIR (mΩ) 85℃ storage retention rate (%) Cycle performance (%) Example 1 31.4 94.3 92.2 Example 2 32.1 93.8 91.8 Example 3 32.3 94.2 92.6 Example 4 31.7 91.4 90.6 Example 5 32.1 92.1 90.8 Example 6 31.2 93.6 91.1 Comparative Example 1 34.1 89.9 78.9 Comparative Example 2 32.2 88.4 77.5 Comparative Example 3 31.9 86.5 76.5 Comparative Example 4 / / / The test results show that the use of diaphragm additives in secondary battery diaphragms can significantly improve the 150°C thermal shrinkage and diaphragm wettability, thereby reducing internal resistance, improving high-temperature cycling, and improving high-rate room-temperature cycling capacity retention.

[0073] By comparing Examples 1-6 and Comparative Examples 1-2, it can be seen that when the diaphragm additive in the present application is applied to the diaphragm, the surface density of the diaphragm can be reduced, the wettability and air permeability of the diaphragm can be improved, and the thermal shrinkage performance of the diaphragm can be improved; when a battery is made using a diaphragm containing the diaphragm additive in the present application, the cycle performance of the battery is improved, so that the battery can still maintain a high capacity after multiple charge and discharge cycles, thereby extending the service life of the battery.

[0074] By comparing Examples 1-6 and Comparative Example 3, it can be seen that when the mass ratio of the vinyl structural unit, the heterocyclic structural unit, the acrylate structural unit and the cross-linking structural unit is (60-85): (5-20): (5-15): (1-15), the performance of the obtained diaphragm additive is better.

[0075] The present invention is further described above with the aid of specific embodiments. However, it should be understood that the specific description here should not be construed as limiting the essence and scope of the present invention. Various modifications made to the above embodiments by ordinary technicians in the field after reading this specification are all within the scope of protection of the present invention.

Claims

1. A membrane additive, characterized in that: The membrane additive includes a polymer, and the polymer includes a vinyl structural unit, a heterocyclic structural unit, an acrylate structural unit and a cross-linking structural unit; the mass ratio of the vinyl structural unit, the heterocyclic structural unit, the acrylate structural unit and the cross-linking structural unit is (60~85): (5~20): (5~15): (1~15); the membrane additive is a fibrous structure, and the aspect ratio of the membrane additive is 5~20.

2. The membrane additive according to claim 1, characterized in that: The length of the membrane additive is 500-2500 nm, and the diameter of the membrane additive is 50-100 nm.

3. The membrane additive according to claim 1, characterized in that: The glass transition temperature of the polymer is ≥150° C., and the swelling degree of the polymer in the electrolyte is 20% to 50%.

4. The membrane additive according to claim 1, characterized in that: The vinyl structural unit is selected from one or more of styrene structural units, vinyl pyrrolidone structural units and vinyl toluene structural units.

5. The membrane additive according to claim 1, characterized in that: The heterocyclic structural unit is selected from one or more of an N-phenylmaleimide structural unit, an isobornyl acrylate structural unit, and an isobornyl methacrylate structural unit.

6. The membrane additive according to claim 1, characterized in that: The acrylic structural unit is selected from one or more of ethyl acrylate structural unit, butyl acrylate structural unit, isooctyl acrylate structural unit, hydroxypropyl acrylate structural unit and hydroxybutyl acrylate structural unit.

7. The membrane additive according to claim 1, characterized in that: The cross-linking structural unit is selected from one or more of polyethylene glycol diacrylate structural units, divinylbenzene structural units, and trimethylolpropane triacrylate structural units.

8. A diaphragm slurry, characterized in that: The diaphragm slurry comprises the diaphragm additive according to any one of claims 1 to 6.

9. A secondary battery separator, characterized in that: The secondary battery separator includes the separator slurry according to claim 7.

10. A battery, characterized in that: The battery comprises the secondary battery separator according to claim 8.

Citation Information

Patent Citations

  • Acrylate functional polymer with photo-initiation active end group and preparation method of polymer

    CN103087234A

  • Novel thermoplastic nanoimprint lithography adhesive as well as synthesis and application methods thereof

    CN103631088A

  • Preparation method of novel 3D printing polyacrylic resin

    CN106749854A

  • PTFE powder, method for producing electrode, and electrode

    CN116134075A