Air-entraining type slurry purifying agent mother liquor as well as preparation method and application thereof
By using air-induced slurry-induced slurry-enhancing large monomers and other gas-induced slurry liquid in concrete, an interpenetrating network structure is formed, which solves the problems of bubble collection and compressive strength reduction, and improves the wrapping properties of concrete and Fullness maintains a high-strength design.
Patent Information
- Application Number
- CN202411026904.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-30
AI Technical Summary
When gas is drawn and slurry is raised in concrete, it is easy to cause bubbles to gather and aggregate, affecting the quality and durability of the project, and increasing the amount of gas drawn will reduce the compressive strength.
Using polyoxyethylene unsaturated large monomers, unsaturated carboxylic acids or anhydrides, sodium alpha-alkenyl sulfonate, monoepoxy terminated unsaturated compounds, crosslinking agents, redox initiation compositions and chain transfer agents The air-induced slurry-extracting agent mother liquor formed an interpenetrating network structure through polymerization, reducing the size of the bubbles and suppressing the upward and convergence of the bubbles.
It significantly improves the encapsulation and fullness of the concrete mixture, maintains the homogeneous dispersion of small bubbles, reduces the bulk weight, ensures the concrete strength design, and avoids the reduction of hardening strength.
Smart Images

Figure QLYQS_1 
Figure BDA0004968800320000071 
Figure BDA0004968800320000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of concrete admixtures, and particularly relates to an air-entraining slurry extracting agent mother liquor and a preparation method and application thereof. Background Art
[0002] Cement concrete technology has experienced nearly 200 years of continuous accumulation, development and improvement. With the rapid development of high-efficiency / high-performance water-reducing agent technology and social progress in the late 1970s, the engineering application of ultra-long, ultra-high and ultra-large volume concrete has become the mainstream of concrete materials. High-performance polycarboxylic acid-based water-reducing agent has become a new generation of concrete admixtures due to its high water-reducing rate, green production raw materials and process. However, in concrete mixtures, changes in ground materials, fine aggregates and mineral powder admixtures often easily lead to bleeding, segregation, and bottoming of fresh concrete materials. Technicians usually improve the fullness of the concrete mixture slurry and the encapsulation of coarse aggregates by improving the water-cement ratio, changing the dosage of water-reducing agent, and using additives (such as adding thickeners and air-entraining agents), thereby improving the working performance of concrete and giving fresh concrete greater fluidity, anti-segregation stability, good filling and other excellent properties.
[0003] Hydroxypropyl methylcellulose, polyacrylic acid polymers and plant gums are often widely used as thickeners or water retaining agents in engineering. The appropriate amount of thickener or water retaining agent components can significantly improve the coating of the slurry on the stone in the concrete mixture, alleviate or improve the segregation and bleeding of concrete, improve the workability and fluidity of the fresh concrete, and improve the stability of the material. However, the interaction between the thickener and cement particles will compete with the interaction between the polycarboxylic acid water reducer and cement particles. In addition, the entanglement between the molecular chains of the thickening components will interfere, which will reduce the effect of the water reducer. The concrete mixture will have a large loss of fluidity in a short time, which is not conducive to construction and pouring. On the other hand, the addition of air entraining agents can improve the fullness and fluidity of the concrete mixture slurry. However, after the concrete mixture containing inferior bubbles is left to stand, transported, loaded and unloaded or poured, most of the small bubbles contained in the material often gather, coalesce, and form large bubbles, which manifests as bubble overflow and floating slurry, seriously affecting the appearance of the project, and endangering the quality and durability of the project. In addition, studies have shown that a 1% increase in the amount of air entrained in concrete will lead to a 5% decrease in its 28d compressive strength, which will directly affect the hardening strength of the concrete and have a negative impact on the concrete structure and durability. Summary of the invention
[0004] The object of the present invention is to provide an air-entraining slurry-raising agent mother solution which can reduce the collection of bubbles while entraining air and slurry-raising in concrete mixtures, as well as a preparation method and application thereof.
[0005] The technical solution of the present invention is as follows:
[0006] An air-entraining pulping agent mother solution has a solid content of 35-45wt% and is prepared from raw materials including the following components in parts by weight:
[0007] 5-50 parts of polyoxyethylene unsaturated macromonomer, 3-30 parts of unsaturated carboxylic acid or / and unsaturated anhydride, 0.3-6 parts of sodium α-olefin sulfonate, 0.003-7 parts of monoepoxy-terminated unsaturated compound, 0.001-2.5 parts of crosslinking agent, 0.3-1.5 parts of redox initiator composition, 0.3-1.5 parts of chain transfer agent and 0.5-91 parts of water;
[0008] The polyoxyethylene unsaturated macromonomer is at least one selected from the group consisting of allyl polyoxyethylene ether, methallyl polyoxyethylene ether, isopentenyl polyoxyethylene ether, polyoxyethylene acrylate, polyoxyethylene methacrylate and isopentenyl polyoxyethylene ester, and the number average molecular weight of the polyoxyethylene unsaturated macromonomer is 500-5000;
[0009] The monoepoxy-terminated unsaturated compound is at least one of allyl glycidyl ether, methyl allyl glycidyl ether, isopentanol glycidyl ether, glycidyl acrylate, glycidyl methacrylate and isopentanol glycidyl ether;
[0010] The crosslinking agent is and / or H2N—X'—NH2, wherein R is H or CH3, R' is H or CH3, and X is (CH2) n1 Chain segment, (CH2CH2O) n2 Segment or ester segment, X' has (CH2) n3 Chain segment, (CH2CH2O) n4 A segment or an ester segment, n1, n2, n3 and n4 are integers;
[0011] In some possible implementations, the raw material further includes 0.01-1 parts by mass of chitosan, and the viscosity of the chitosan is 10-500 mPa·s.
[0012] In some possible implementations, the crosslinking agent is selected from at least one of diethanol dimethacrylate, polyethylene glycol dimethacrylate, 1,6-hexanediol dimethacrylate and 1,6-hexanediol dimethacrylate, diallyl glycol ether, diallyl polyethylene glycol ether, ethylenediamine, triethylene glycol diamine, decanediamine and butanediamine.
[0013] In some possible implementations, the redox initiator composition includes an oxidant and a reductant, the oxidant is ammonium persulfate and / or peroxide, and the reductant is Fe 2+ and / or vitamin C, the mass ratio of the oxidant to the reductant is 1.5-3.75:1.
[0014] In some possible implementations, the chain transfer agent is mercaptoacetic acid and / or mercaptopropionic acid, and the mass ratio of the chain transfer agent to the reducing agent is 1:1.2-4.
[0015] In some possible implementations, the unsaturated carboxylic acid is selected from at least one of acrylic acid, methacrylic acid and maleic acid;
[0016] The unsaturated acid anhydride is at least one selected from acrylic anhydride, methacrylic anhydride and maleic anhydride.
[0017] A method for preparing the above-mentioned air-entraining type pulping agent mother liquor comprises the following steps:
[0018] (1) dissolving 3-90% of a polyoxyethylene unsaturated macromonomer, 5-75% of an unsaturated carboxylic acid or / and an unsaturated anhydride, 0-50% of a monoepoxy-terminated unsaturated compound, 0-100% of sodium α-olefin sulfonate and a portion of a crosslinking agent in an appropriate amount of water, adding 30-70% of a redox initiator composition and 30-70% of a chain transfer agent in batches at room temperature, controlling the temperature of the reaction system to be no greater than 60° C., adding a portion of the crosslinking agent after the temperature of the reaction system begins to drop, and until the temperature of the reaction system begins to drop significantly, to obtain a solution of a first intermediate, wherein the total amount of the crosslinking agent added in step (1) is 25-85%;
[0019] (2) adding the remaining amount of polyoxyethylene unsaturated macromonomer, unsaturated carboxylic acid and / or unsaturated anhydride, monoepoxy-terminated unsaturated compound, sodium α-olefin sulfonate, part of the crosslinking agent and appropriate amount of water to the first intermediate solution, adding the remaining amount of redox initiator composition and chain transfer agent at 30° C., controlling the temperature of the reaction system to be no greater than 60° C., adding the remaining amount of crosslinking agent after the temperature of the reaction system begins to drop, and waiting for the temperature of the reaction system to drop to room temperature to obtain a second intermediate solution;
[0020] (3) adjusting the solid content of the solution of the second intermediate to 35-45 wt % to obtain an air-entraining type pulping agent mother solution having an interpenetrating network structure;
[0021] In some possible implementations, the raw material further comprises 0.01-1 parts by weight of chitosan, and the viscosity of the chitosan is 10-500 mPa·s;
[0022] Chitosan is added in at least one of step (1), step (2) and step (3).
[0023] A concrete slurry-addition composition comprises the above-mentioned air-entraining slurry-addition agent mother liquor.
[0024] The present invention has at least the following beneficial effects:
[0025] 1. The raw materials of the mother solution of the air-entraining slurry-raising agent of the present invention form an interpenetrating network structure through polymerization reaction. After being used in concrete, it can significantly improve the encapsulation of the concrete mixture slurry, reduce the size of the air droplets, inhibit the process of floating, escaping and agglomeration of tiny air droplets through the gap between aggregates, improve and maintain the uniform dispersion of small air droplets in the concrete, improve the workability and workability of the concrete, and significantly reduce the bulk density of the concrete mixture while ensuring the design grade of concrete strength.
[0026] 2. In some possible implementations, chitosan participates in the formation of an interpenetrating network or is modified on the interpenetrating network, which can further improve the water retention and strength of concrete.
[0027] 3. The concrete slurry composition obtained by compounding the air-entraining slurry agent mother solution of the present invention with other components is mixed into concrete, which improves the fullness of the concrete mixture slurry without reducing the hardening strength of the concrete. In addition, compared with the concrete slurry composition obtained by compounding with the existing triterpene saponin air-entraining agent, no additional thickener is required. DETAILED DESCRIPTION
[0028] The technical solution of the present invention is further illustrated and described below through specific implementation methods.
[0029] In the following examples, the water used can be one or more of distilled water, purified water, drinking water, and tap water; unless otherwise specified, the detection methods in the following examples are conventional detection methods; the reagents in the following examples are purchased from commercial channels unless otherwise specified.
[0030] The deacetylation degree of chitosan used in the following examples is 85%. In other possible embodiments, the deacetylation degree of chitosan is 85%-100%.
[0031] The high-performance polycarboxylate water-reducing agent mother liquor used in the following examples is ZS-M90M produced by Zhongshi (Fujian) New Building Materials Technology Co., Ltd.; the organosilicon defoamer used in the following examples is organosilicon defoamer 611-c; the triterpenoid saponin air-entraining agent is also a commercially available product; the thickener is HPMC with a viscosity of 100,000 to 200,000 (aq).
[0032] Example 1
[0033] (1) 120 g of isopentanol polyoxyethylene ether, 200 g of methallyl polyoxyethylene ether, 55 g of acrylic acid, and 4.8 g of ethylene glycol dimethacrylate are dispersed and dissolved in 400 g of water. After stirring and dissolving evenly, a redox initiator composition (0.85 g of hydrogen peroxide, 0.5 g of vitamin C) and 1.1 g of mercaptopropionic acid are added dropwise to the monomer mixed solution in batches to initiate an aqueous phase polymerization reaction. The temperature of the reaction system is controlled to be no more than 60° C., and the temperature of the reaction system begins to drop significantly to obtain a first intermediate solution.
[0034] (2) A mixed solution of 230 g of isopentanol polyoxyethylene ether, 100 g of acrylic acid, 1.6 g of dimethyl acrylate-1,6-hexanediol ester, 1.8 g of glycidyl acrylate, 48 g of sodium α-olefin sulfonate and 220 g of water was added to the first intermediate solution under stirring. After stirring and dissolving evenly, a redox initiator composition (2.9 g of hydrogen peroxide, 1 g of vitamin C) and a chain transfer agent 2.9 g of mercaptopropionic acid were added dropwise to the monomer mixed solution in batches to initiate a polymerization reaction. The temperature of the reaction system was controlled to be no more than 60° C. After the temperature of the reaction system began to drop, the pH was adjusted to neutral, and then 0.8 g of ethylenediamine was added. The stirring was continued until the temperature of the reaction system began to drop significantly, thereby obtaining a second intermediate solution.
[0035] (3) Adding an appropriate amount of water to adjust the solid content of the second intermediate solution to 40 wt % to obtain an air-entraining type pulping agent mother solution with an interpenetrating network structure.
[0036] Example 2
[0037] (1) 280 g of prenol polyoxyethylene ether, 60 g of acrylic acid, 10 g of maleic anhydride, and 6 g of polyethylene glycol dimethacrylate (polyethylene glycol M n =200), 40g of sodium α-olefin sulfonate was dissolved in 450g of water, and after stirring and dissolving evenly, a redox initiator composition (1.7g of hydrogen peroxide, 7g of vitamin C) and 2g of mercaptopropionic acid were added dropwise in batches to the mixed solution of the monomers to initiate a polymerization reaction. The temperature of the reaction system was controlled to be no more than 60°C, and when the temperature of the reaction system began to drop significantly, a first intermediate solution was obtained.
[0038] (2) A mixed solution of 410 g of isopentanol polyoxyethylene ether, 60 g of acrylic acid, 2.8 g of glycidyl methacrylate, and 127.2 g of water was added to the first intermediate solution under stirring, and after stirring evenly, a redox initiator composition (1.7 g of hydrogen peroxide, 0.7 g of vitamin C) and 2 g of mercaptopropionic acid were added dropwise to the monomer mixed solution in batches, and the temperature of the reaction system was controlled to be no more than 60° C. After the temperature of the reaction system began to drop, the pH was adjusted to neutral, and then 100 g of an aqueous solution containing 1.2 g of triethylene glycol diamine and 0.8 g of chitosan was added, and stirring was continued until the temperature of the reaction system dropped to room temperature to obtain a second intermediate solution.
[0039] (3) adding an appropriate amount of water to adjust the solid content of the second intermediate solution to 40 wt % to obtain a mother solution of a cross-linked air-entraining type pulping agent; the viscosity of the chitosan used is 150 mPa·s.
[0040] Example 3
[0041] (1) 280 g of isopentanol polyoxyethylene ether, 70 g of acrylic acid, 3 g of dimethacrylate-1,6-hexanediol ester, and 40 g of sodium α-olefin sulfonate are dissolved in 260 g of water. After stirring and dissolving evenly, a redox initiator composition (1.5 g of hydrogen peroxide, 0.7 g of vitamin C) and 1 g of mercaptopropionic acid are added dropwise to the aqueous solution of the mixed monomers in batches to initiate a polymerization reaction. The temperature of the reaction system is controlled to be no more than 60° C., and the temperature of the reaction system begins to drop significantly to obtain a first intermediate solution.
[0042] (2) A mixed solution of 110 g of isopentanyl polyoxyethylene ether, 200 g of methallyl polyoxyethylene ester, 50 g of acrylic acid, 10 g of methacrylic acid, 3.2 g of allyl glycidyl ether and 176.8 g of water was added to the first intermediate solution under stirring, and after stirring evenly, a redox initiator composition (1.5 g of hydrogen peroxide, 0.7 g of vitamin C) and 1 g of mercaptopropionic acid were added dropwise to the monomer mixed solution in batches, and the temperature of the reaction system was controlled to be no more than 60° C. After the temperature of the reaction system began to drop, the pH was adjusted to neutral, and then 200 g of a chitosan aqueous solution was added, the chitosan aqueous solution containing 3.2 g of chitosan with a viscosity of 150 mPa·s was added, and stirring was continued until the temperature of the reaction system dropped to room temperature to obtain a second intermediate solution.
[0043] (3) Adding an appropriate amount of water to adjust the solid content of the second intermediate solution to 40 wt % to obtain an air-entraining type pulping agent mother solution with an interpenetrating network structure.
[0044] Example 4
[0045] (1) 300 g of isopentyl polyoxyethylene ether, 55 g of acrylic acid, 6 g of allyl glycidyl ether and 15 g of sodium α-olefin sulfonate were dissolved in 400 g of water, and after being stirred and dissolved uniformly at room temperature, a redox initiator composition (2.5 g of hydrogen peroxide, 1.2 g of vitamin C) and 2.8 g of mercaptopropionic acid were added dropwise to the monomer mixed solution in batches to initiate a polymerization reaction, and the temperature of the reaction system was controlled to be no more than 60° C. After the temperature of the reaction system began to drop, the pH was adjusted to neutral, and then 10 g of decanediamine was added until the temperature of the reaction system began to drop significantly, thereby obtaining a first intermediate solution.
[0046] (2) A mixed solution of 300 g of isopentanol polyoxyethylene ether, 50 g of acrylic acid, 15 g of maleic acid, 5.8 g of isopentanol glycidyl ether and 25 g of sodium α-olefin sulfonate in 54.2 g of water was added to the first intermediate solution under stirring, and after stirring evenly, a redox initiator composition (2.5 g of hydrogen peroxide, 1.2 g of vitamin C) and 2.8 g of mercaptopropionic acid were added dropwise to the monomer mixed solution in batches to initiate a polymerization reaction and control the temperature of the reaction system to be no more than 60° C. After the temperature of the reaction system began to drop, the pH was adjusted to neutral, and then 2 g of ethylenediamine and 4.5 g of water-soluble chitosan (viscosity 300 mPa·s) were added. The mixture was stirred continuously until the temperature of the reaction system dropped to room temperature to obtain a second intermediate solution.
[0047] (3) Adding an appropriate amount of water to adjust the solid content of the second intermediate solution to 40 wt % to obtain an air-entraining type pulping agent mother solution with an interpenetrating network structure.
[0048] Example 5
[0049] (1) 50 g of acrylic acid, 140 g of isopentenyl polyoxyethylene ether, 2 g of dimethacrylate-1,6-hexanediol ester, and 70 g of sodium α-olefin sulfonate were dissolved in 260 g of water, and after being stirred and dissolved uniformly, a redox initiator composition (2 g of hydrogen peroxide, 0.9 g of vitamin C) and 1.5 g of mercaptopropionic acid were used as chain transfer agents to initiate the polymerization reaction of the monomers, and the reaction temperature was controlled not to exceed 60° C. After the temperature of the reaction materials began to drop significantly, a first intermediate solution was obtained.
[0050] (2) Add 250 g of isopentanol polyoxyethylene ether, 200 g of polyoxyethylene acrylate, 65 g of acrylic acid, 3.2 g of glycidyl methacrylate and 433 g of water to the first intermediate solution under stirring, stir evenly, and then dropwise add the redox initiator composition (2.5 g of hydrogen peroxide, 1.5 g of vitamin C) and 1.8 g of mercaptopropionic acid to the monomer mixed solution in batches to initiate polymerization reaction, control the temperature of the reaction system to be no more than 60° C., adjust the pH to neutral after the temperature of the reaction system starts to drop, then add 0.6 g of diaminobutane and 200 g of chitosan aqueous solution, wherein the chitosan aqueous solution contains 2.5 g of chitosan with a viscosity of 200 mPa·s, continue stirring, and wait for the temperature of the reaction system to drop to room temperature to obtain a second intermediate solution.
[0051] (3) Adding an appropriate amount of water to adjust the solid content of the second intermediate solution to 40 wt % to obtain an air-entraining type pulping agent mother solution with an interpenetrating network structure.
[0052] Performance test: concrete slurry composition and its performance test
[0053] Example 6-10: The interpenetrating network structure of the air-entraining slurry agent mother liquor prepared in Example 1-Example 5 was synthesized and used as a concrete slurry addition composition after the air-entraining slurry agent mother liquor, high-performance water-reducing mother liquor, sodium gluconate, defoamer and water were compounded in a mass ratio of 3-10:22:1:0.02:69-78; at the same time, commercially available air-entraining agents and thickening slurry components were selected for comparison to obtain a compounded concrete slurry addition composition.
[0054] Comparative Examples 1-4: The slurry extract composition of the comparison group was obtained by compounding the high-performance carboxylic acid water-reducing agent mother liquor, triterpenoid saponin air-entraining agent, thickener, sodium gluconate, silicone defoaming agent and water in a mass ratio of 22:0-0.8:0-1:1:0.02:75.2-76.7.
[0055] The specific compositions and proportions of Examples 6-10 and Comparative Examples 1-4 are shown in Table 1:
[0056] Table 1 Raw materials and mass ratios of Examples 6-10 and 1-4
[0057]
[0058] Examples 6-10 and Comparative Examples 1-4 were added to C30 concrete, and concrete trial mixing tests were conducted on C30 concrete mixed with concrete slurry extracting compositions of different compositions. The test method was based on GB / T50080-2016, and the bulk density and concrete specimen strength at 7d and 28d were tested. The results are shown in Table 2:
[0059] Table 2 Comparison of concrete bulk density and strength of concrete grouting compositions with different compositions
[0060]
[0061] As can be seen from Table 2, the concrete-added slurry composition obtained by compounding the air-entraining slurry extracting agent mother solution of the present invention with other components and mixing it into concrete can improve the fullness of the concrete mixture slurry, reduce the concrete bulk density and improve its compressive strength without reducing the hardened strength of the concrete.
[0062] The above are only preferred embodiments of the present invention, and therefore cannot be used to limit the scope of implementation of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.
Claims
1. An air-entraining type pulping agent mother solution, characterized in that: The solid content is 35-45 wt% and is prepared from raw materials including the following components in parts by weight: 5-50 parts of polyoxyethylene unsaturated macromonomer, 3-30 parts of unsaturated carboxylic acid or / and unsaturated anhydride, 0.3-6 parts of sodium α-olefin sulfonate, 0.003-7 parts of monoepoxy-terminated unsaturated compound, 0.001-2.5 parts of crosslinking agent, 0.3-1.5 parts of redox initiator composition, 0.3-1.5 parts of chain transfer agent and 0.5-91 parts of water; The polyoxyethylene unsaturated macromonomer is at least one selected from the group consisting of allyl polyoxyethylene ether, methallyl polyoxyethylene ether, isopentenyl polyoxyethylene ether, polyoxyethylene acrylate, polyoxyethylene methacrylate and polyoxyethylene isopentenyl acid, and the number average molecular weight of the polyoxyethylene unsaturated macromonomer is 500-5000; The monoepoxy-terminated unsaturated compound is at least one of allyl glycidyl ether, methyl allyl glycidyl ether, isopentanol glycidyl ether, glycidyl acrylate, glycidyl methacrylate and isopentanol glycidyl ether; The crosslinking agent is and / or H2N—X'—NH2, wherein R is H or CH3, R' is H or CH3, and X is (CH2) n1 Chain segment, (CH2CH2O) n2 Segment or ester segment, X' has (CH2) n3 Chain segment, (CH2CH2O) n4 A segment or an ester segment, n1, n2, n3 and n4 are integers.
2. The air-entraining type pulping agent mother solution according to claim 1, characterized in that: The raw materials also include 0.01-1 parts by mass of chitosan, and the viscosity of the chitosan is 10-500 mPa·s.
3. The air-entraining type pulping agent mother solution according to claim 1, characterized in that: The crosslinking agent is selected from at least one of diethanol dimethacrylate, polyethylene glycol dimethacrylate, 1,6-hexanediol dimethacrylate and 1,6-hexanediol dimethacrylate, diallyl glycol ether, diallyl polyethylene glycol ether, ethylenediamine, triethylene glycol diamine, decanediamine and butanediamine.
4. The air-entraining type pulping agent mother solution according to claim 1, characterized in that: The redox initiator composition comprises an oxidant and a reductant, wherein the oxidant is ammonium persulfate and / or peroxide, and the reductant is Fe 2+ and / or vitamin C, the mass ratio of the oxidant to the reductant is 1.5-3.75:
1.
5. The air-entraining type pulping agent mother solution according to claim 4, characterized in that: The chain transfer agent is mercaptoacetic acid and / or mercaptopropionic acid, and the mass ratio of the chain transfer agent to the reducing agent is 1:1.2-4.
6. The air-entraining type pulping agent mother solution according to claim 1, characterized in that: The unsaturated carboxylic acid is selected from at least one of acrylic acid, methacrylic acid and maleic acid; The unsaturated acid anhydride is at least one selected from acrylic anhydride, methacrylic anhydride and maleic anhydride.
7. A method for preparing an air-entraining type stock-lifting agent mother solution as claimed in any one of claims 1 to 6, characterized in that: The steps include: (1) dissolving 3-90% of a polyoxyethylene unsaturated macromonomer, 5-75% of an unsaturated carboxylic acid or / and an unsaturated anhydride, 0-50% of a monoepoxy-terminated unsaturated compound, 0-100% of sodium α-olefin sulfonate and part of a cross-linking agent in an appropriate amount of water, adding 30-70% of a redox initiator composition and 30-70% of a chain transfer agent in batches at room temperature, controlling the temperature of the reaction system to be no greater than 60° C., adding part of the cross-linking agent after the temperature of the reaction system begins to drop, and until the temperature of the reaction system begins to drop significantly, to obtain a solution of a first intermediate, wherein the total amount of the cross-linking agent added in step (1) is 25-85%; (2) adding the remaining amount of the polyoxyethylene unsaturated macromonomer, the unsaturated carboxylic acid or the unsaturated acid anhydride, the monoepoxy-terminated unsaturated compound, the sodium α-olefin sulfonate, a portion of the cross-linking agent and an appropriate amount of water to the first intermediate solution, adding the remaining amount of the redox initiator composition and the chain transfer agent at 30° C., controlling the temperature of the reaction system to be no greater than 60° C., adding the remaining amount of the cross-linking agent after the temperature of the reaction system begins to drop, and waiting for the temperature of the reaction system to drop to room temperature to obtain a second intermediate solution; (3) adjusting the solid content of the solution of the second intermediate to 35-45 wt % to obtain the mother solution of the air-entraining type pulping agent with the interpenetrating network structure.
8. The preparation method according to claim 7, characterized in that: The raw materials also include 0.01-1 parts by weight of chitosan, wherein the viscosity of the chitosan is 10-500 mPa·s; The chitosan is added in at least one of step (1), step (2) and step (3).
9. A concrete slurry addition composition, characterized in that: The invention comprises the air-entraining pulping agent mother liquor as described in any one of claims 1 to 6.
Citation Information
Patent Citations
Special super-plasticizer for manufactured sand concrete and preparation method thereof
CN110283329A
Polycarboxylate concrete air entraining agent and preparation method thereof
CN111777719A
Hyperbranched concrete tackifier as well as preparation method and application thereof
CN113637123A
Foam-stabilizing polycarboxylic acid slump retaining agent as well as preparation method and application thereof
CN118085188A
Polycarboxylic acid type copolymer and method for producing the same, and use of the same