Organosilicon modified acrylic emulsion, water-based heat insulation coating, water-based heat reflection finishing coat and preparation method thereof

The combination of silicone modified acrylic emulsion with infrared reflective pigment and hollow glass microbeads is made into aqueous thermal reflection thermal insulation and anticorrosion coatings, which solves the environmental pollution and adhesion problems of existing thermal reflection coatings and achieves efficient thermal energy reflection and thermal insulation effect, and reduce energy consumption and environmental pollution.

CN118930762APending Publication Date: 2024-11-12MARINE CHEM RES INST CO LTD

Patent Information

Application Number
CN202410685623.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-25
Filing Date
2024-05-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing thermal reflective coatings have environmental pollution problems, the infrared reflectivity is not ideal, and it is prone to absorb water in high humidity or rainy days, resulting in a decrease in thermal conductivity, which cannot meet the adhesion requirements of buildings and storage tanks to thermal insulation coatings.

Method used

The adhesion and weather resistance of the resin are improved by combining silicone modified acrylic emulsion with infrared reflective pigments, hollow glass microbeads, etc., and the adhesion and weather resistance of the resin are improved by copolymerizing silane prepolymers and unsaturated monomers, and Water is used as a medium during the preparation process to reduce VOC content.

Benefits of technology

Achieve 50-80% solar thermal energy reflection, significantly reduces the temperature in the room or container, improves the water resistance and adhesion of the coating, meets the heat insulation and corrosion protection needs of buildings and storage tanks, and replaces solvent-based thermal reflective coatings. Save energy and improve the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004866867120000101
    Figure BDA0004866867120000101
  • Figure BDA0004866867120000151
    Figure BDA0004866867120000151
  • Figure BDA0004866867120000191
    Figure BDA0004866867120000191
Patent Text Reader

Abstract

The invention discloses an organic silicon modified acrylic emulsion, a water-based heat insulation coating, a water-based heat reflection finishing coat and a preparation method thereof, and relates to the technical field of anticorrosive coatings. The organic silicon modified acrylic emulsion is obtained by copolymerizing the following raw materials: a silane prepolymer, styrene, an unsaturated monomer, an emulsifier, a water-soluble initiator, softened water, an oil-soluble initiator and a reducing agent, the silane prepolymer contains an unsaturated double bond and an alkoxy group. According to the invention, the silane coupling agent and the unsaturated monomer are copolymerized and connected to a main chain of a polymer, so that the adhesion of resin to pigments and fillers, especially hollow glass beads, is improved, and the dry-state and wet-state adhesion of a primer to a substrate and the dry-state and wet-state adhesion of a finish paint to the primer are improved; in addition, the weather resistance and the heat resistance of the paint film are improved by modifying the organic silicon resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of anti-corrosion coatings, and more particularly to an organosilicon-modified acrylic emulsion, a water-based heat-insulating coating, a water-based heat-reflecting topcoat and a preparation method thereof. Background Art

[0002] Ordinary paints, especially dark paints, absorb infrared rays in sunlight and convert them into heat energy, causing the coating temperature to rise. The heat is then transferred from the coating to the substrate, and then from the substrate to the inner wall, causing the temperature in the room or container to rise, causing discomfort in indoor work and life in summer or increased air conditioning energy consumption, or bringing about oil storage tank safety issues. Heavy oil, residual oil, and wax oil have high viscosity at low temperatures and are not easy to transport. Therefore, they need to be heated to reach and maintain an appropriate temperature. In order to prevent heat loss, the storage tanks and pipelines need to be insulated.

[0003] Traditional insulation materials are generally profiles, including inorganic insulation profiles based on inorganic porous materials such as mineral wool, glass wool, and expanded perlite, and organic foam boards based on polystyrene and polyurethane foam materials. The former has the advantage of being non-flammable, but its disadvantage is that it has poor waterproofing effect, will form thermal bridges due to water absorption on rainy days, greatly reduce the insulation performance, and also affect the anti-corrosion performance of the coating. The latter has the disadvantages of being flammable and not resistant to organic solvents. Moreover, although the foam profile itself has good water resistance, it has many joints and is easy to seep water in the gaps, resulting in poor waterproofing and board shedding.

[0004] For the heat reflection of the roof, the traditional method is to stick aluminum foil on the surface of the waterproof layer or use waterproof coiled materials with aluminum foil. For the heat reflection treatment of storage tanks, silver paint was mainly used in the past. The aluminum of the aluminum foil or the silver powder in the silver paint will be corroded due to surface oxidation, and the reflective ability will decrease. In the 1990s, the United States developed high-performance heat insulation coatings based on the principle of spacecraft surface insulation materials. It has been promoted and applied in building roofs, petrochemical storage tanks and pipelines, ship hulls and superstructure insulation coatings. Compared with ordinary coatings, this coating can reflect or scatter more infrared rays, which plays a role in isolating solar heat. Used in light oil storage tanks can significantly reduce the temperature in open-air storage tanks in summer and improve safety.

[0005] Most of the existing heat-reflective coatings are solvent-based coatings. For example, Japanese patent JP98-120946 publicly introduces a dark-colored infrared reflective coating, which is composed of a combination of metal oxide black pigments, indium phosphide, flaky aluminum powder, fluororesin, and polysulfone resin. Its infrared reflectivity is 31% and its weather resistance is excellent. The disadvantage is that the base material is a solvent-based resin, which has environmental pollution problems, and its infrared reflectivity is not ideal. German patent DE19501114 introduces an infrared reflective coating, which is based on water-diluted acrylic resin, titanium dioxide, chrome black, iron red and other pigments, talcum powder, mica powder and other fillers, and is applied on a white primer to form a coating with a dry film thickness of 45μm, and the infrared heat reflectivity is >50%. The disadvantage of this coating is that it uses a mixture of ether alcohol and water as a diluent, which still has environmental pollution problems.

[0006] Chinese patent 201510105180.4 discloses a water-based thermal insulation coating, the components of which are: perlite, vermiculite, acrylic emulsion, bactericide and mildewproof agent, thickener, and plasticizer; the component ratio is: 15% perlite, 65% vermiculite, 15% acrylic emulsion, 0.4% bactericide and mildewproof agent, 4% thickener, and 0.6% plasticizer. The implementation method is: perlite and vermiculite are mixed into a mixture, and the remaining components are mixed into a mixed liquid, and the two are mixed and stirred into a slurry. It has a low cost and is suitable for thermal insulation of internal and external walls of buildings. The thermal insulation coating made by this method must be prepared and used immediately, because the fluffy structure of perlite and vermiculite is easily destroyed by water, and there is also a problem that the coating film is easy to absorb water, resulting in a decrease in the thermal insulation effect of the coating. Chinese patent 20151040 9852.0 discloses a building wall thermal insulation coating, which is a composite of a barrier-type thermal insulation coating with a heat barrier function and a reflective thermal insulation coating with a heat reflective function. The barrier-type thermal insulation coating is based on heat-insulating lightweight aggregate fly ash beads, ceramic microbeads, etc., and is compounded with resin emulsion, functional fillers, etc.: bulk density ≤500kg / m 3, thermal conductivity 0.035-0.06W / (m·k). Reflective thermal insulation coatings are based on reflective fillers and functional pigments, and are compounded with resin emulsions, functional fillers, etc. This patent uses power plant floating beads, which are low in cost and suitable for building wall insulation, but the strength of power plant floating beads is not high and is not very suitable for tank insulation and anti-corrosion. In order to improve the thermal insulation performance, the thermal insulation coatings of existing inventions all use a large volume percentage of thermal insulation fillers and polymer emulsions. The thermal insulation fillers used include expanded perlite, power plant floating beads, hollow glass microspheres, aerogels, etc. The emulsions used include acrylic emulsions, ethylene-vinyl acetate copolymer emulsions, etc. The thermal insulation coatings using expanded perlite and expanded vermiculite powder have low costs, but poor thermal insulation performance. They are easy to absorb water on rainy days or in high humidity environments, resulting in a significant decrease in thermal conductivity. The thermal insulation coating using aerogel can achieve higher thermal insulation performance in a dry state, but it also has the problem of easy water absorption, resulting in a decrease in thermal conductivity, and is not suitable for outdoor thermal insulation coatings. The polymer emulsion used in the existing thermal insulation coating is ordinary acrylic emulsion or ethylene-vinyl acetate copolymer emulsion, and the dry and wet adhesion of the paint film cannot meet the requirements of some coastal oil storage tank customers for the adhesion of thermal insulation coating. Summary of the invention

[0007] In order to solve the problems existing in the prior art, the present invention provides an organosilicon-modified acrylic emulsion, a water-based heat-insulating coating, a water-based heat-reflecting topcoat and a preparation method thereof. The present invention uses the organosilicon-modified acrylic emulsion as a base material, and is combined with infrared reflective pigments, hollow glass microspheres, additives, etc. to prepare a water-based heat-reflecting heat-insulating anticorrosive coating, and its construction performance, drying performance, paint film mechanical properties, decorative properties, anticorrosive properties, heat reflection and heat insulation properties all reach or exceed the level of solvent-based heat-reflective coatings.

[0008] One of the purposes of the present invention is to provide a silicone-modified acrylic emulsion.

[0009] The organosilicon-modified acrylic emulsion of the present invention is obtained by copolymerizing raw materials including the following components:

[0010] Silane prepolymer, styrene, unsaturated monomer, emulsifier, water-soluble initiator, softened water, oil-soluble initiator and reducing agent;

[0011] Each component is calculated by weight:

[0012] Styrene 100 parts by weight;

[0013] Silane prepolymer 5-25 parts by weight, preferably 10-20 parts by weight;

[0014] 80-125 parts by weight of unsaturated monomer, preferably 90-120 parts by weight;

[0015] Emulsifier 8-15 parts by weight, preferably 10-12 parts by weight;

[0016] 1-4 parts by weight, preferably 1-2 parts by weight, of a water-soluble initiator;

[0017] 220-280 parts by weight of softened water, preferably 230-260 parts by weight;

[0018] 3-5 parts by weight, preferably 4-5 parts by weight, of an oil-soluble initiator;

[0019] 0.5-2 parts by weight, preferably 0.5-1 parts by weight, of a reducing agent;

[0020] The silane prepolymer contains an unsaturated double bond and an alkoxy group.

[0021] In a preferred embodiment of the present invention, the silane prepolymer is prepared by the following method:

[0022] After heating the silane coupling agent, silicate monomer, isopropanol and ion exchange resin for reaction, water is added dropwise for stirring and reaction, and the silane prepolymer is obtained after standing;

[0023] Each component is calculated by weight:

[0024] 100 parts by weight of silane coupling agent;

[0025] 50-150 parts by weight of silicate monomer, preferably 60-120 parts by weight;

[0026] 20-40 parts by weight of isopropanol, preferably 25-35 parts by weight;

[0027] 4-10 parts by weight of ion exchange resin, preferably 5-7 parts by weight;

[0028] Water: 6-18 parts by weight, preferably 10-15 parts by weight.

[0029] In a preferred embodiment of the present invention,

[0030] The silane coupling agent is at least one of glycidyloxypropyl trimethoxysilane (6040 silane coupling agent), glycidyloxypropyl triethoxysilane, methacryloxypropyl trimethoxysilane (570 silane coupling agent), methacryloxypropyl triethoxysilane, vinyl triethoxysilane, vinyl trimethoxysilane, and vinyl tris (β-methoxyethoxy) silane; and / or,

[0031] The silicate monomer is at least one of tetraethyl silicate, diethyl methylphenyl silicate, diethyl diphenyl silicate, triethyl methyl silicate and diethyl dimethyl silicate; and / or,

[0032] The ion exchange resin is a strongly acidic ion exchange resin, which is a commonly used ion exchange resin in the art, such as IR1000NA and 15WET ion exchange resins from Dow, C100E and CT175 ion exchange resins from Purolite, D001*7 ion exchange resins from Shanghai Kaiping Resin, CT-500 ion exchange resins from Jiangsu Secosai Resin, etc.; and / or,

[0033] The water is deionized water. Preferably, the conductivity of the water is ≤20 μs / cm.

[0034] In a preferred embodiment of the present invention,

[0035] The reaction temperature of the temperature-raising reaction is 60-65° C., and / or the stirring speed is 50-150 rpm, and / or the reaction time is 5-10 minutes; and / or,

[0036] The water is added dropwise for 1-1.5 hours; and / or,

[0037] The reaction time of the stirring reaction is 1-1.5 hours; and / or,

[0038] The standing time is more than 12 hours.

[0039] In a preferred embodiment of the present invention,

[0040] The unsaturated monomer is an acrylic acid monomer or versatile vinyl carbonate; preferably, the acrylic acid monomer is at least one of acrylic acid, methacrylic acid, methyl methacrylate, glycidyl acrylate, butyl acrylate, butyl methacrylate, and octyl acrylate; and / or, the versatile vinyl carbonate is C9-11 versatile vinyl carbonate, and / or,

[0041] The emulsifier is an ionic emulsifier and a nonionic emulsifier; preferably, the weight ratio of the ionic emulsifier to the nonionic emulsifier is (1-4):1, preferably (1-2):1; more preferably, the ionic emulsifier is at least one of alkylphenol ether sodium succinate sulfonate (such as MS-1 emulsifier), sodium lauryl sulfate (SDS emulsifier), alkylphenol ether phosphate (TXP-10 emulsifier), and / or, the nonionic emulsifier is alkylphenol polyether or alkyl alcohol polyether (such as OP-10 emulsifier, OP-15 emulsifier, TX-10 emulsifier, TX-15 emulsifier, OS-15 emulsifier); and / or,

[0042] The water-soluble initiator is a persulfate, preferably ammonium persulfate or potassium persulfate; and / or,

[0043] The oil-soluble initiator is at least one of benzoyl peroxide, tert-butyl peroxide and dicumyl peroxide; and / or,

[0044] Among them, water-soluble initiators are used for emulsion polymerization, and oil-soluble initiators and reducing agents are used in combination to initiate the copolymerization of silane prepolymers and unsaturated monomers, while eliminating residual monomers.

[0045] The softened water is deionized water or distilled water. Preferably, the conductivity of the softened water is ≤20 μs / cm; and / or,

[0046] The reducing agent is at least one of sodium formaldehyde sulfoxylate, sodium bisulfite, and ascorbic acid.

[0047] A second object of the present invention is to provide a method for preparing a silicone-modified acrylic emulsion.

[0048] The preparation method of the organosilicon-modified acrylic emulsion of the present invention comprises:

[0049] A portion of softened water, a portion of an emulsifier, styrene and an unsaturated monomer are mixed and stirred for emulsification to obtain a pre-emulsion; the remaining softened water, the remaining emulsifier, a portion of the pre-emulsion and a portion of a water-soluble initiator solution are subjected to a first temperature-raising reaction under a protective gas atmosphere; the temperature is continued to be raised, the remaining pre-emulsion is added dropwise, and the remaining water-soluble initiator solution is added in batches for a second temperature-raising reaction; after cooling, a silane prepolymer, an oil-soluble initiator solution and a reducing agent solution are added in sequence under stirring for a cooling reaction, and the organosilicon-modified acrylic emulsion is obtained after the pH is adjusted.

[0050] There is no particular limitation on the part of softened water, part of emulsifier, part of the pre-emulsion, and part of water-soluble initiator solution in the above steps. The technicians add them according to the actual situation in order to make the reaction proceed fully. The total amount can meet the limitation of the present invention.

[0051] In a preferred embodiment of the present invention,

[0052] The water-soluble initiator solution is a solution prepared by dissolving the water-soluble initiator in the softened water. Preferably, the concentration of the water-soluble initiator solution is 4-6 wt %; and / or,

[0053] The solvent of the oil-soluble initiator solution is isopropanol or propylene glycol methyl ether. Preferably, the concentration of the oil-soluble initiator solution is 40-60 wt %; and / or,

[0054] The reducing agent solution is a solution prepared by dissolving the reducing agent in the softened water. Preferably, the concentration of the reducing agent solution is 4-6 wt %; and / or,

[0055] The stirring emulsification time is 15-30 minutes, and / or the stirring speed is 800-1200 rpm; and / or,

[0056] The reaction temperature of the first temperature-raising reaction is 72-78° C., and / or, the first temperature-raising reaction is performed until the reaction system turns blue; and / or,

[0057] The remaining pre-emulsion is added dropwise for 1.5-2 hours, and / or the remaining initiator solution is added dropwise evenly or in 3-5 batches, and a batch of initiator solution is added every half an hour or so, and / or the reaction temperature of the second temperature-raising reaction is 80-85° C., and / or the reaction time of the second temperature-raising reaction is 0.5-1 hour; and / or,

[0058] The dropping time of the reducing agent solution is 0.5-1h, and / or the reaction temperature of the cooling reaction is 50-60°C, and / or the reaction time of the cooling reaction is 0.5-1 hour; and / or,

[0059] The pH after adjustment is 7-8.

[0060] The following solutions can be adopted:

[0061] ① Add part of softened water, part of ionic emulsifier, part of nonionic emulsifier, a mixture of styrene and acrylic monomers into an emulsification container, stir and emulsify at 800-1200 rpm for 15-30 minutes to obtain a pre-emulsion;

[0062] ② Add the remaining softened water, the remaining ionic emulsifier, the remaining non-ionic emulsifier, part of the pre-emulsion, and part of the water-soluble initiator solution into the reaction container, raise the temperature to 72-78°C, pass nitrogen, and keep warm until the liquid turns blue;

[0063] ③ Raise the temperature to 80-85°C, gradually add the remaining pre-emulsion dropwise, add it within 1.5-2 hours, and at the same time add the remaining water-soluble initiator solution in three batches, continue to keep warm and react for 0.5-1 hour after adding;

[0064] ④ Cool down to 50-60℃, add silane prepolymer while stirring, then add oil-soluble initiator solution, stir well and drop reducing agent solution, add all within 0.5-1h, and continue to keep warm for 0.5-1h after adding;

[0065] ⑤ Add a neutralizing agent to adjust the pH value of the emulsion to 7-8 to obtain the organosilicon-modified acrylic emulsion.

[0066] Wherein, the neutralizing agent is a volatile base, preferably ammonia water or an organic amine, more preferably AMP-95, 2-amino-1-propanol, N-methylmorpholine, N-ethylmorpholine, N,N-dimethylethanolamine (DMEA), triethylamine, etc., and its molar amount is 80-100% of the molar amount of carboxyl groups in the unsaturated monomer.

[0067] A third object of the present invention is to provide a water-based thermal insulation coating.

[0068] The water-based thermal insulation coating of the present invention is prepared from raw materials including the following components:

[0069] Silicone-modified acrylic emulsion, film-forming aid, pigment, filler, hollow glass microsphere, additive, thickener and softened water;

[0070] Each component is calculated by weight:

[0071] 100 parts by weight of silicone-modified acrylic emulsion;

[0072] 5-8 parts by weight of film-forming aid, preferably 6-7 parts by weight;

[0073] Pigment 10-50 parts by weight, preferably 30-40 parts by weight;

[0074] Filler 25-70 parts by weight, preferably 30-50 parts by weight;

[0075] 30-60 parts by weight, preferably 40-50 parts by weight, of hollow glass microspheres;

[0076] 2.5-10 parts by weight of auxiliary agent, preferably 3-6 parts by weight;

[0077] Thickener 0.6-1.5 parts by weight, preferably 0.8-1.2 parts by weight;

[0078] 50-80 parts by weight of demineralized water, preferably 60-70 parts by weight.

[0079] In a preferred embodiment of the present invention,

[0080] The film-forming aid is at least one of dodecyl alcohol ester, hexadecanol ester, dipropylene glycol monobutyl ether, and tripropylene glycol monobutyl ether; and / or,

[0081] The infrared absorption rate of the pigment is ≤50%, and / or the infrared reflectivity is ≥25%; preferably, the pigment is at least one of titanium dioxide, titanium nickel yellow, and iron oxide yellow; and / or,

[0082] The filler is at least one of fine talc powder, heavy calcium carbonate, precipitated barium sulfate, silicon powder, and magnesium hydroxide; and / or,

[0083] The hollow glass microspheres are non-porous hollow structures. Preferably, the particle size of the hollow glass microspheres is 20-120 μm, and / or the true density is 0.15-0.4 g / cm 3 and / or,

[0084] The auxiliary agent is at least one of a dispersant, a wetting agent, a leveling agent, a defoamer, a mildewproof agent, and a preservative; wherein the dispersant is a commonly used dispersant in the art, and its selection is usually determined by the properties of the pigment. For inorganic pigments such as titanium dioxide, ammonium and potassium salts of copolymers of olefin monomers and unsaturated carboxylic acids and their esters can be used, such as: Nopco's 5027 and 5029 dispersants, COATEX's BR3 dispersant, Hemmings' FX-600 dispersant, Hankook Chemical's HT-5020 dispersant, and Saifei Chemical's DS-195 dispersant, and its dosage is 1-3% of the amount of pigment used; the wetting agent is a commonly used wetting agent in the art, and polyether-modified acetylenic alcohols can be used, such as SURFYNOL GA and SURFYNOL TG, Tianjin Saifei's SF-340 wetting agent, the dosage of which is 0.1-0.3% of the total amount of water-based thermal insulation coating; the leveling agent is a commonly used leveling agent in this field, and silane-modified polyether or fluorocarbon-modified polyether can be used, such as Byk348 of Germany's BYK, EFKA-3570 of the Netherlands' Efka, and 245, 270, and 4100 leveling agents of Degao; the defoamer is a commonly used defoamer in this field, and mineral oil polyether defoamers or polyether-modified silicone defoamers can be used, such as SN-1370 and NXZ of Nopco, BYK 024 of BYK, and 810 and 825 defoamers of Degao, and the dosage is 0.05-0.2% of the total amount of water-based thermal insulation coating; the mildew inhibitor is a commonly used mildew inhibitor in this field, and Dow's SKANE M-8 mildewproof agent, TROY 689 mildewproof agent, SK MA-21 mildewproof agent, the amount of which is 0.1-0.5% of the total amount of water-based thermal insulation coating; preservatives are commonly used preservatives in the field, such as KATHON LXE preservative from Oriental-Rohm and Haas Company and 531 preservative from Baoding Sunshine, the amount of which is 0.1-0.3% of the total amount of water-based thermal insulation coating; and / or,

[0085] The thickener is a commonly used thickener in the art, preferably a polyether thickener or an alkali-soluble acrylic emulsion thickener; the polyether thickener is such as Dow's RM-8W thickener and Hemmings' R-278 thickener; the alkali-soluble acrylic emulsion thickener is such as Dow's TT-935 thickener; and / or,

[0086] The softened water is deionized water or distilled water. Preferably, the conductivity of the softened water is ≤20 μs / cm.

[0087] A fourth object of the present invention is to provide a method for preparing a water-based thermal insulation coating.

[0088] The preparation method of the water-based thermal insulation coating of the present invention comprises:

[0089] Softened water, additives, pigments, fillers and part of thickeners are mixed and ground to obtain a color paste, and the color paste, silicone-modified acrylic emulsion, hollow glass microbeads and the remaining thickener are mixed, and the pH value is adjusted and then filtered to obtain the water-based thermal insulation coating.

[0090] The thickener in the above steps is not particularly limited, and the technicians add it according to the actual situation, the purpose is to make the reaction proceed fully, and the total amount can meet the definition of the present invention.

[0091] The following solutions can be adopted:

[0092] ① Add measured softened water and additives into the slurry preparation container and stir evenly with an adjustable high-speed disperser;

[0093] ②Add pigments and fillers and disperse at high speed to the required fineness;

[0094] ③ Add some thickener, stir well to obtain color paste;

[0095] ④ Add color paste, silicone-modified acrylic emulsion and hollow glass microbeads into the paint mixing container and stir well;

[0096] ⑤Add the remaining thickener and stir well;

[0097] ⑥Add pH regulator to adjust the pH value to 8-10;

[0098] ⑦Filter, package and obtain the finished product.

[0099] The pH adjuster is a volatile base, preferably ammonia or an organic amine, more preferably AMP-95, 2-amino-1-propanol, N-methylmorpholine, N-ethylmorpholine, N,N-dimethylethanolamine (DMEA), triethylamine, etc.

[0100] In the actual preparation process, silicone-modified acrylic emulsion can be used in combination with commercially available styrene-acrylic emulsion and commercially available pure acrylic emulsion (XG-2001 emulsion, XG-666 emulsion, etc.), which can further reduce costs while ensuring the quality of the finished product.

[0101] A fifth object of the present invention is to provide a water-based heat-reflective topcoat.

[0102] The water-based heat-reflective topcoat of the present invention is prepared from raw materials including the following components:

[0103] Silicone-modified acrylic emulsion, film-forming aid, pigment, filler, hollow glass microsphere, covering polymer, heat-reflective titanium dioxide, additives, thickener and softened water;

[0104] Each component is calculated by weight:

[0105] 100 parts by weight of silicone-modified acrylic emulsion;

[0106] 5-8 parts by weight, preferably 5-7 parts by weight, of a film-forming aid;

[0107] Pigment 0-20 parts by weight, preferably 5-18 parts by weight;

[0108]

[0109] In a preferred embodiment of the present invention,

[0110] The film-forming aid is at least one of dodecyl alcohol ester, hexadecanol ester, dipropylene glycol monobutyl ether, and tripropylene glycol monobutyl ether; and / or,

[0111] The infrared absorptivity of the pigment is ≤50%, and / or the infrared reflectivity is ≥25%; preferably, the pigment is at least one of iron oxide red, iron oxide yellow, titanium nickel yellow, cobalt blue, phthalocyanine blue, chromium oxide green, iron chrome black, and perylene black; and / or,

[0112] The filler is at least one of fine talc powder, ultrafine calcium carbonate, precipitated barium sulfate, silicon powder, and magnesium hydroxide; and / or,

[0113] The hollow glass microspheres are non-porous hollow structures. Preferably, the particle size of the hollow glass microspheres is 20-120 μm, and / or the true density is 0.15-0.4 g / cm 3 ; For example, 3M's S-15, K-20, K25 glass microspheres, Anhui Kaisheng's 18P1000, 20P1000, 25P1500 glass microspheres; and / or,

[0114] The covering polymer is a polymer emulsion containing polymer hollow microspheres, which can form closed micropores after the paint film dries and has good covering power. Specifically, Dow's ULTRA-E covering polymer emulsion and Wanhua's H-400 covering polymer emulsion can be used; and / or,

[0115] The heat-reflective titanium dioxide is a rod-shaped rutile titanium dioxide. Preferably, the heat-reflective titanium dioxide has a short diameter of 0.3-0.5 μm and / or a long diameter of 2-4 μm. The titanium dioxide with a special crystal size selected in the present invention has the characteristics of low tinting strength and high infrared reflectivity. Specifically, Huntsman's Altiris 550, 800 thermal insulation titanium dioxide and Ishihara's PFR 404 thermal insulation titanium dioxide can be used. And / or,

[0116] The auxiliary agent is at least one of a dispersant, a wetting agent, a leveling agent, a defoamer, a mildew preventer, and a preservative; wherein the dispersant is a commonly used dispersant in the art, and its selection is usually determined by the properties of the pigment. For inorganic pigments such as red iron oxide, ammonium and potassium salts of copolymers of olefin monomers and unsaturated carboxylic acids and their esters can be used, such as: Nopco's 5040, 5027, 5029 dispersants, COATEX's BR3 dispersant, Hemmings' FX-600 dispersant, Hankook Chemical's HT-5020 dispersant Powder, DS-195 dispersant from Saifei Chemical, the dosage of which is 1-3% of the amount of pigment; for organic pigments such as phthalocyanine blue, copolymerized acrylic acid ammonium salt or potassium salt, or high molecular block copolymer with pigment-friendly groups can be used, such as Byk190 dispersant from Germany's BYK, EFKA-4550 dispersant from the Netherlands' Efka, 123K dispersant from COATEX, 7500W dispersant from Hemmings, 5027, 5029, 6130 dispersants from Nopco, HT A10 dispersant from Hankook Chemical, DS-194L dispersant from Saifei Chemical, the dosage of which is 10-30% of the amount of pigment; the wetting agent is a wetting agent commonly used in this field, and polyether-modified acetylenic alcohol can be used, such as SURFYNOL GA and SURFYNOL from American Gas Chemical Company. TG, Tianjin Saifei's SF-340 wetting agent, the dosage of which is 0.1-0.3% of the total amount of water-based heat reflective topcoat; the leveling agent is a commonly used leveling agent in this field, and silane-modified polyether or fluorocarbon-modified polyether can be used, such as Byk348 of Germany's BYK, EFKA-3570 of the Netherlands' Efka, and 245, 270, and 4100 leveling agents of Degao; the defoamer is a commonly used defoamer in this field, and mineral oil polyethers or polyether-modified silicones can be used, such as Hemmings' 7010 and 7015 defoamers, Nopco's SN-1311, SN-1370, and NXZ defoamers, BYK 024 of BYK, and Degao's 810 and 825 defoamers, and the dosage is 0.05-0.2% of the total amount of water-based heat reflective topcoat; the mildew inhibitor is a commonly used mildew inhibitor in this field, and Dow's SKANE M-8 mildewcide, TROY 689 mildewcide, SK MA-21 mildewcide, the amount of which is 0.1-0.5% of the total amount of water-based heat reflective topcoat; the preservative is a preservative commonly used in the art, such as isothiazolinone preservatives, specifically KATHON LXE preservative from Oriental-Rohm and Haas Company and 531 preservative from Baoding Sunshine, the amount of which is 0.1-0.3% of the total amount of water-based heat reflective topcoat; and / or,

[0117] The thickener is a commonly used thickener in the art, preferably a polyether thickener or an alkali-soluble acrylic emulsion thickener; the polyether thickener is such as Dow's RM-8W thickener, Hemmings' R-278 thickener, Rh-278 thickener; the alkali-soluble acrylic emulsion thickener is such as Dow's TT-935 thickener; and / or,

[0118] The softened water is deionized water or distilled water. Preferably, the conductivity of the softened water is ≤20 μs / cm.

[0119] The sixth object of the present invention is to provide a method for preparing a water-based heat-reflective topcoat.

[0120] The preparation method of the water-based heat-reflective topcoat of the present invention comprises:

[0121] Softened water, additives, pigments, fillers, heat-reflective titanium dioxide and part of thickener are mixed and ground to obtain a color paste, and the color paste, silicone-modified acrylic emulsion, covering polymer, hollow glass microspheres and remaining thickener are mixed, and the pH is adjusted and then filtered to obtain the water-based heat-reflective topcoat.

[0122] The thickener in the above steps is not particularly limited, and the technicians add it according to the actual situation, the purpose is to make the reaction proceed fully, and the total amount can meet the definition of the present invention.

[0123] The following solutions can be adopted:

[0124] ① Add measured softened water and additives into the slurry preparation container and stir evenly with an adjustable high-speed disperser;

[0125] ② Add pigment, filler, heat-reflective titanium dioxide, and disperse at high speed for 20 minutes;

[0126] ③ Grind to required fineness;

[0127] ④ Add some thickener, stir well to obtain color paste;

[0128] ⑤ Add color paste and silicone-modified acrylic emulsion into the paint mixing container and stir well;

[0129] ⑥Add covering polymer and hollow glass microspheres, stir at medium speed;

[0130] ⑦Add the remaining thickener and stir well;

[0131] ⑧Add pH regulator to adjust the pH value to 8-9;

[0132] ⑨Filter, package and obtain the finished product.

[0133] The pH adjuster is a volatile base, preferably ammonia or an organic amine, more preferably AMP-95, 2-amino-1-propanol, N-methylmorpholine, N-ethylmorpholine, N,N-dimethylethanolamine (DMEA), triethylamine, etc.

[0134] Beneficial effects:

[0135] The uniqueness of the organosilicon-modified acrylic emulsion of the present invention lies in that: firstly, the silane coupling agent is copolymerized with the unsaturated monomer and inserted into the polymer main chain, thereby improving the adhesion of the resin to the pigment, filler, especially the hollow glass microspheres, and improving the dry and wet adhesion of the primer to the substrate and the topcoat to the primer; secondly, the modification of the organosilicon resin by the present invention improves the weather resistance and heat resistance of the paint film.

[0136] Compared with common coatings and existing solvent-based heat-reflective coatings, the present invention has the following advantages:

[0137] ①Excellent heat reflection and heat insulation performance. This water-based heat reflective paint can reflect 50-80% of solar heat energy and significantly reduce the temperature in the room or container.

[0138] ② Safe and convenient to use. This paint uses water as the medium and has a low VOC content, which improves the construction environment and avoids fire hazards.

[0139] ③Good decorative effect. The particle size of the emulsion is small, which can obtain a uniform, fine and highly decorative topcoat.

[0140] ④ The paint film has good comprehensive performance. The base material of this coating is a core-shell structured silicone-modified acrylic emulsion. The silicone segment of its shell can greatly improve the weather resistance of the coating. The hydrolyzable alkoxy group can improve the adhesion between the emulsion and the pigment filler, especially the hollow glass microspheres, and significantly improve the water resistance of the coating and the adhesion to the substrate. Due to the synergistic effect of acrylic resin and silicone resin, the paint film has the excellent construction and quick drying properties of acrylic resin and the heat resistance and weather resistance of silicone resin. The resulting coating has a dense film, and the paint film has excellent adhesion, mechanical properties, water resistance, alkali resistance, and weather resistance.

[0141] The present invention has broad application prospects. All technical indicators of the coating have reached the level of solvent-based heat-reflective coatings, and can completely replace solvent-based heat-reflective coatings. It has been proven that the coating has good practical effects in reflecting and isolating solar heat on the roofs and inner and outer walls of buildings, storage tanks and pipelines in petrochemical plants, trains, ships and other facilities, and reducing internal temperatures. Replacing ordinary protective coatings or solvent-based heat-reflective heat-insulating coatings with the water-based heat-reflective heat-insulating coating of the present invention can save energy, protect the environment, and achieve huge social benefits and considerable economic benefits. The implementation of the present invention not only has significant economic benefits, but also has huge social benefits. It is of great significance to the technological progress of the energy-saving and environmentally friendly materials industry, as well as to the protection and improvement of the ecological environment. DETAILED DESCRIPTION

[0142] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0143] The raw materials used in the present invention are all commercially available products.

[0144] Example 1

[0145] The silane prepolymer was prepared according to the formula in Table 1 below:

[0146] Add diethyl methylphenyl silicate, 570 silane coupling agent (methacryloxypropyltrimethoxysilane), isopropanol and ion exchange resin CT175 into a four-necked flask, heat to 60°C, and stir at 50-150 rpm for 5 minutes; add water dropwise during stirring, and the addition is completed within 1.5 hours. After the addition, continue to keep warm and stir for 1 hour, let it stand overnight, and the product is a transparent solution.

[0147] Example 2

[0148] The silane prepolymer was prepared according to the formula in Table 1 below:

[0149] Add diethyl methylphenyl silicate, 570 silane coupling agent, isopropanol and ion exchange resin CT-500 into a four-necked flask, raise the temperature to 60°C, and stir at a low speed of 50-150 rpm for 5 minutes; add water dropwise during stirring, and the addition shall be completed within 1.2 hours. After the addition, continue to keep warm and stir for 1 hour, and let it stand overnight. The product is a transparent solution.

[0150] Example 3

[0151] The silane prepolymers were prepared according to the formulas in Table 1 below:

[0152] Add diethyl methylphenyl silicate, 570 silane coupling agent, 6040 silane coupling agent (glycidyloxypropyltrimethoxysilane), isopropanol and ion exchange resin CT-500 into a four-necked flask, raise the temperature to 60°C, and stir at a low speed of 50-150 rpm for 5 minutes; add water dropwise during stirring, and the addition shall be completed within 1 hour. After the addition, continue to keep warm and stir for 1 hour, and let it stand overnight. The product is a transparent solution.

[0153] Example 4

[0154] The silane prepolymers were prepared according to the formulas in Table 1 below:

[0155] Add diethyl methylphenyl silicate, tetraethyl silicate, 570 silane coupling agent, isopropanol and ion exchange resin D001*7 into a four-necked flask, raise the temperature to 60°C, and stir at a low speed of 50-150 rpm for 5 minutes; add water dropwise during stirring, and the addition shall be completed within 1 hour. After the addition, continue to keep warm and stir for 1 hour, and let it stand overnight. The product is a transparent solution.

[0156] Example 5

[0157] The silane prepolymers were prepared according to the formulas in Table 1 below:

[0158] Add diethyl methylphenyl silicate, 570 silane coupling agent, isopropanol and ion exchange resin D001*7 into a four-necked flask, raise the temperature to 60°C, and stir at a low speed of 50-150 rpm for 5 minutes; add water dropwise during stirring, and the addition shall be completed within 1 hour. After the addition, continue to keep warm and stir for 1 hour, and let it stand overnight. The product is a transparent solution.

[0159] Table 1

[0160]

[0161] Example 6

[0162] The silicone-modified acrylic emulsion was prepared according to the formula in Table 2 below:

[0163] ① Add 370 g of softened water, 10 g of MS-1 emulsifier, 10 g of TX-10 emulsifier, and 440 g of a mixture of methacrylic acid, styrene, and butyl acrylate into a beaker, stir at a high speed of 800-1200 rpm, and stir and emulsify for 15 minutes to obtain a pre-emulsion;

[0164] ② Add 50 g of softened water, 10 g of MS-1 emulsifier, 150 g of pre-emulsion, and 15 g of 5% ammonium persulfate solution into the reaction vessel, raise the temperature to 72-78°C, pass nitrogen, and keep warm until the liquid turns blue;

[0165] ③ Raise the temperature to 80-85℃, gradually add the remaining pre-emulsion solution dropwise within 1.5-2h, and add the remaining ammonium persulfate solution in three batches at the same time. Continue to keep warm for 0.5h after adding;

[0166] ④ Cool down to 50-60°C, add the silane prepolymer prepared in Example 1 while stirring, then add 50% propylene glycol methyl ether solution of tert-butyl peroxide, stir well and add dropwise 5% sodium bisulfite solution, add all within 0.5-1h, and keep warm for 0.5h after addition.

[0167] ⑤Add ammonia water, stir evenly, and adjust the pH to 7-8.

[0168] Example 7

[0169] The silicone-modified acrylic emulsion was prepared according to the formula in Table 2 below:

[0170] ① Add 370 g of softened water, 4 g of MS-1 emulsifier, 8 g of TX-10 emulsifier, and 440 g of a mixture of methacrylic acid, styrene, and butyl acrylate into a beaker, stir and emulsify at 800-1200 rpm for 15 minutes to obtain a pre-emulsion;

[0171] ② Add 50 g of softened water, 4 g of MS-1 emulsifier, 150 g of pre-emulsion, and 15 g of 5% potassium persulfate solution into the reaction vessel, raise the temperature to 72-78°C, pass nitrogen, and keep warm until the liquid turns blue;

[0172] ③ Raise the temperature to 80-85℃, gradually add the remaining pre-emulsion solution dropwise within 1.5-2h, and add the remaining potassium persulfate solution in three batches at the same time. Continue to keep warm for 0.5h after adding;

[0173] ④ Cool down to 50-60°C, add the silane prepolymer prepared in Example 1 while stirring, then add 50% propylene glycol methyl ether solution of tert-butyl peroxide, stir well and add dropwise 5% sodium bisulfite solution, add all within 0.5-1h, and keep warm for 0.5h after addition.

[0174] ⑤Add ammonia water, stir evenly, and adjust the pH to 7-8.

[0175] Example 8

[0176] The silicone-modified acrylic emulsion was prepared according to the formula in Table 2 below:

[0177] ① Add 370 g of softened water, 10 g of TXP-10 emulsifier, 10 g of TX-10 emulsifier, and 430 g of a mixture of acrylic acid, styrene, and butyl acrylate into a beaker, stir and emulsify at 800-1200 rpm for 15 minutes to obtain a pre-emulsion;

[0178] ② Add 50g of softened water, 10g of TXP-10 emulsifier, 150g of pre-emulsion, and 15g of 5% ammonium persulfate solution into the reaction vessel, raise the temperature to 72-78°C, pass nitrogen, and keep warm until the liquid turns blue;

[0179] ③ Raise the temperature to 80-85℃, gradually add the remaining pre-emulsion solution dropwise within 1.5-2h, and add the remaining ammonium persulfate solution in three batches at the same time. Continue to keep warm for 0.5h after adding;

[0180] ④ Cool down to 50-60°C, add the silane prepolymer prepared in Example 1 while stirring, then add 50% propylene glycol methyl ether solution of tert-butyl peroxide, stir well and add dropwise 5% sodium formaldehyde sulfoxylate solution, add all within 0.5-1h, and keep warm for 0.5h after addition.

[0181] ⑤Add DMEA, stir evenly and adjust the pH to 7-8.

[0182] Example 9

[0183] The silicone-modified acrylic emulsion was prepared according to the formula in Table 2 below:

[0184] ① Add 370 g of softened water, 5 g of MS-1 emulsifier, 15 g of TX-10 emulsifier, and 440 g of a mixture of methacrylic acid, acrylic acid, styrene, and butyl acrylate into a beaker, stir and emulsify at 800-1200 rpm for 15 minutes to obtain a pre-emulsion;

[0185] ② Add 50 g of softened water, 10 g of MS-1 emulsifier, 150 g of pre-emulsion, and 15 g of 5% potassium persulfate solution into the reaction vessel, raise the temperature to 72-78°C, pass nitrogen, and keep warm until the liquid turns blue;

[0186] ③ Raise the temperature to 80-85℃, gradually add the remaining pre-emulsion solution dropwise within 1.5-2h, and add the remaining potassium persulfate solution in three batches at the same time. Continue to keep warm for 0.5h after adding;

[0187] ④ Cool down to 50-60°C, add the silane prepolymer prepared in Example 1 while stirring, then add 50% propylene glycol methyl ether solution of benzoyl peroxide, stir well and add dropwise 5% sodium formaldehyde sulfoxylate solution, add all within 0.5-1h, and keep warm for 0.5h after addition.

[0188] ⑤Add DMEA, stir evenly and adjust the pH to 7-8.

[0189] Example 10

[0190] The silicone-modified acrylic emulsion was prepared according to the formula in Table 2 below:

[0191] ① Add 370 g of softened water, 5 g of sodium lauryl sulfate, 10 g of OS-15 emulsifier, and 440 g of a mixture of methacrylic acid, acrylic acid, styrene and butyl acrylate into a beaker, stir and emulsify at 800-1200 rpm for 15 minutes to obtain a pre-emulsion;

[0192] ② Add 50 g of softened water, 5 g of sodium lauryl sulfate, 150 g of pre-emulsion, and 15 g of 5% ammonium persulfate solution into the reaction vessel, raise the temperature to 72-78°C, pass nitrogen, and keep warm until the liquid turns blue;

[0193] ③ Raise the temperature to 80-85℃, gradually add the remaining pre-emulsion solution dropwise within 1.5-2h, and add the remaining ammonium persulfate solution in three batches at the same time. Continue to keep warm for 0.5h after adding;

[0194] ④ Cool down to 50-60°C, add the silane prepolymer prepared in Example 2 while stirring, then add 50% propylene glycol methyl ether solution of benzoyl peroxide, stir well and add 5% ascorbic acid solution dropwise, add within 0.5-1h, and keep warm for 0.5 hour after addition.

[0195] ⑤Add 2-amino-1-propanol, stir evenly, and adjust the pH to 7-8.

[0196] Embodiment 11

[0197] The silicone-modified acrylic emulsion was prepared according to the formula in Table 2 below:

[0198] ① Add 350 g of softened water, 10 g of OS-15 emulsifier, 5 g of sodium lauryl sulfate, and 432 g of a mixture of methacrylic acid, styrene, and butyl acrylate into a beaker, stir and emulsify at 800-1200 rpm for 15 minutes to obtain a pre-emulsion;

[0199] ② Add 40 g of softened water, 10 g of sodium lauryl sulfate, 150 g of pre-emulsion, and 15 g of 5% potassium persulfate solution into the reaction vessel, raise the temperature to 72-78°C, pass nitrogen, and keep warm until the liquid turns blue;

[0200] ③ Raise the temperature to 80-85℃, gradually add the remaining pre-emulsion solution dropwise within 1.5-2h, and add the remaining potassium persulfate solution in three batches at the same time. Continue to keep warm for 0.5h after adding;

[0201] ④ Cool down to 50-60°C, add the silane prepolymer prepared in Example 1 while stirring, then add 50% propylene glycol methyl ether solution of benzoyl peroxide, stir well and add 5% ascorbic acid solution dropwise, add within 0.5-1h, and keep warm for 0.5 hour after addition.

[0202] ⑤Add 2-amino-1-propanol, stir evenly, and adjust the pH to 7-8.

[0203] Table 2

[0204]

[0205] The following performance tests were performed on the organosilicon-modified acrylic emulsions prepared in Examples 6-11 above. The specific results are shown in Table 3 below.

[0206] Table 3

[0207]

[0208] The mechanical stability in Table 3 is tested according to the method specified in GB / T 20623. If there is no demulsification and no obvious floccules, it is considered to have passed. The calcium ion stability is tested according to the method specified in GB / T 20623. If there is no stratification, no sinking, and no flocculation after 48 hours, it is considered to have passed. The water resistance of the paint film is tested according to the method specified in GB / T 1733. If there is no bubbling, wrinkling, or shedding after immersion for 48 hours, it is considered to have passed.

[0209] Examples 12-17

[0210] The water-based thermal insulation coatings were prepared according to the formulas in Table 4 below. The preparation process is as follows:

[0211] ① Add measured softened water, wetting agent, defoamer, preservative, mildew preventer and other additives into the slurry preparation container, use an adjustable high-speed disperser, speed 300-500 rpm, stir for 5-10 minutes;

[0212] ② Add pigments such as titanium dioxide, yellow iron oxide, magnesium hydroxide, ultrafine calcium hydroxide and other fillers, 800-1200 rpm, high-speed dispersion for 30-50 minutes;

[0213] ③ Add 1 / 3 of the formula amount of thickener, stir well, and prepare color paste;

[0214] ④ Add the above color paste, silicone-modified acrylic emulsion, film-forming aid, and hollow glass microspheres into the paint mixing container, and stir at medium speed at 500-800 rpm for 10-20 minutes;

[0215] ⑤Add the remaining thickener and stir at high speed for 20-30 minutes;

[0216] ⑥Add triethylamine or other pH regulator to adjust the pH value to 8-10;

[0217] ⑦Filter, package and obtain the finished product.

[0218] Examples 12-17 use homemade silicone-modified acrylic emulsion as the base material; the amount of hollow glass microspheres used ranges from 13% to 15% of the total weight of the coating.

[0219] Comparative Example 1

[0220] The amount of hollow glass microspheres used in Comparative Example 1 is 10% of the total weight of the coating. It can be seen from the test data in Table 5 that the thermal conductivity thereof decreases significantly.

[0221] Comparative Example 2

[0222] The preparation method of Comparative Example 2 is the same as that of Examples 12-17, except that the organosilicon-modified acrylic emulsion is replaced by commercially available acrylic emulsions such as XG-2001 emulsion and XG-666 emulsion.

[0223] It can be seen from the test data in Table 5 that the acid resistance of the coating is poor.

[0224] Table 4

[0225]

[0226] The titanium dioxide is rutile type, with infrared absorption rate ≤0.05 and infrared thermal reflectivity greater than or equal to 0.80; the infrared absorption rate of iron oxide yellow is ≤0.25 and infrared reflectivity is ≥0.6; the particle size of K-20 hollow microspheres is 30-110μm, and the actual density is about 0.2g / cm 3 .

[0227] The water-based thermal insulation coatings prepared in the above Examples 12-17 and the coatings prepared in Comparative Examples 1 and 2 were subjected to performance tests as shown in Table 5 below. The test results are shown in Table 6 below.

[0228] Table 5

[0229]

[0230] Table 6

[0231]

[0232] Examples 18-23

[0233] The water-based heat-reflective topcoat was prepared according to the formula in Table 7 below. The preparation process is as follows:

[0234] ① Add measured softened water, wetting agent, dispersant, preservative, mildew inhibitor, defoamer and other additives into the slurry preparation container, use an adjustable high-speed disperser, speed 300-500 rpm, and stir at low speed for 3-5 minutes;

[0235] ② Add pigments such as iron oxide yellow, iron chrome black, magnesium hydroxide, ultrafine calcium hydroxide and other fillers, heat reflective titanium dioxide, and disperse at high speed for 20 minutes;

[0236] ③ Grind to a fineness of ≤40μm;

[0237] ④Add 1 / 3 of the formula amount of thickener, stir well to obtain color paste;

[0238] ⑤ Add the above color paste, silicone-modified acrylic emulsion and film-forming aid into the paint mixing container, stir at 500-800 rpm for 10-20 minutes;

[0239] ⑥Add covering polymer and hollow glass microspheres, 500-800 rpm, stir for 10-20 minutes;

[0240] ⑦Add the remaining thickener, 800-1200 rpm, stir for 20-30 minutes;

[0241] ⑧ Add triethylamine or other pH regulator to adjust the pH value to 8-9;

[0242] ⑨Filter, package and obtain the finished product.

[0243] Comparative Example 3

[0244] The preparation method of Comparative Example 3 is the same as that of Examples 18-23, except that the pigment, the covering polymer and the heat-reflecting titanium dioxide are replaced by silver paste.

[0245] It can be seen from the test data in Table 9 that its thermal reflectivity is lower than that of the water-based thermal reflective topcoat of Example 23 with similar brightness.

[0246] Comparative Example 4

[0247] The preparation method of Comparative Example 4 is the same as that of Examples 18-23, except that the acrylic emulsion therein is replaced with commercially available acrylic emulsions such as XG-2001 emulsion and AC-261 emulsion.

[0248] It can be seen from the test data in Table 7 that the water resistance of the coating is poor.

[0249] Comparative Example 5

[0250] The preparation method of Comparative Example 5 is the same as that of Examples 18-23, except that the pigment is replaced by black iron oxide. It can be seen from the test data in Table 7 that its thermal reflectivity is significantly lower than that of iron chrome black pigment.

[0251] Table 7

[0252]

[0253]

[0254] Among them, 404 titanium dioxide is aluminum-coated rod-shaped particles with a long diameter of 2-4μm, a short diameter of 0.3-0.5μm, an infrared absorptivity of ≤0.05, and an infrared thermal reflectivity of ≥0.85; the infrared absorptivity of iron oxide yellow is ≤0.25, and the infrared reflectivity is ≥0.6; the infrared absorptivity of iron chrome black is ≤0.45, and the infrared reflectivity is ≥0.38; the particle size of K-20 hollow microspheres is 30-110μm, and the true density is about 0.2g / cm 3 .

[0255] The water-based heat-reflective topcoats prepared in the above Examples 18-23 and the coatings prepared in Comparative Examples 3-5 were subjected to the performance tests shown in Table 8 below. The test results are shown in Table 9 below.

[0256] Table 8

[0257]

[0258] Table 9

[0259]

Claims

1. A silicone-modified acrylic emulsion, characterized in that The organosilicon-modified acrylic emulsion is obtained by copolymerizing raw materials including the following components: Silane prepolymer, styrene, unsaturated monomer, emulsifier, water-soluble initiator, softened water, oil-soluble initiator and reducing agent; Each component is calculated by weight: Styrene 100 parts by weight; Silane prepolymer 5-25 parts by weight, preferably 10-20 parts by weight; 80-125 parts by weight of unsaturated monomer, preferably 90-120 parts by weight; Emulsifier 8-15 parts by weight, preferably 10-12 parts by weight; 1-4 parts by weight, preferably 1-2 parts by weight, of a water-soluble initiator; 220-280 parts by weight of softened water, preferably 230-260 parts by weight; 3-5 parts by weight, preferably 4-5 parts by weight, of an oil-soluble initiator; 0.5-2 parts by weight, preferably 0.5-1 parts by weight, of a reducing agent; The silane prepolymer contains an unsaturated double bond and an alkoxy group.

2. The organosilicon-modified acrylic emulsion according to claim 1, characterized in that The silane prepolymer is prepared by the following method: After heating the silane coupling agent, silicate monomer, isopropanol and ion exchange resin for reaction, water is added dropwise for stirring and reaction, and the silane prepolymer is obtained after standing; Each component is calculated by weight: 100 parts by weight of silane coupling agent; 50-150 parts by weight of silicate monomer, preferably 60-120 parts by weight; 20-40 parts by weight of isopropanol, preferably 25-35 parts by weight; 4-10 parts by weight of ion exchange resin, preferably 5-7 parts by weight; Water: 6-18 parts by weight, preferably 10-15 parts by weight.

3. The organosilicon-modified acrylic emulsion according to claim 2, characterized in that: The silane coupling agent is at least one of glycidyloxypropyl trimethoxysilane, glycidyloxypropyl triethoxysilane, methacryloxypropyl trimethoxysilane, methacryloxypropyl triethoxysilane, vinyl triethoxysilane, vinyl trimethoxysilane, and vinyl tris(β-methoxyethoxy)silane; and / or, The silicate monomer is at least one of tetraethyl silicate, diethyl methylphenyl silicate, diethyl diphenyl silicate, triethyl methyl silicate and diethyl dimethyl silicate; and / or, The ion exchange resin is a strongly acidic ion exchange resin; and / or, The water is deionized water. Preferably, the conductivity of the water is ≤20 μs / cm.

4. The organosilicon-modified acrylic emulsion according to claim 2, characterized in that: The reaction temperature of the temperature-raising reaction is 60-65° C., and / or the stirring speed is 50-150 rpm, and / or the reaction time is 5-10 minutes; and / or, The water is added dropwise for 1-1.5 hours; and / or, The reaction time of the stirring reaction is 1-1.5 hours; and / or, The standing time is more than 12 hours.

5. The organosilicon-modified acrylic emulsion according to claim 1, characterized in that: The unsaturated monomer is an acrylic acid monomer or versatile vinyl carbonate. Preferably, the acrylic acid monomer is at least one of acrylic acid, methacrylic acid, methyl methacrylate, glycidyl acrylate, butyl acrylate, butyl methacrylate, and octyl acrylate; preferably, the versatile vinyl carbonate is C9-11 versatile vinyl carbonate; and / or, The emulsifier is an ionic emulsifier and a nonionic emulsifier; preferably, the weight ratio of the ionic emulsifier to the nonionic emulsifier is (1-4):1, preferably (1-2):1; more preferably, the ionic emulsifier is at least one of sodium alkylphenol ether succinate sulfonate, sodium lauryl sulfate, and alkylphenol ether phosphate, and / or, the nonionic emulsifier is alkylphenol polyether or alkyl alcohol polyether; and / or, The water-soluble initiator is a persulfate, preferably ammonium persulfate or potassium persulfate; and / or, The oil-soluble initiator is at least one of benzoyl peroxide, tert-butyl peroxide and dicumyl peroxide; and / or, The softened water is deionized water or distilled water. Preferably, the conductivity of the softened water is ≤20 μs / cm; and / or, The reducing agent is at least one of sodium formaldehyde sulfoxylate, sodium bisulfite, and ascorbic acid.

6. A method for preparing the organosilicon-modified acrylic emulsion according to any one of claims 1 to 5, characterized in that The method comprises: A portion of softened water, a portion of an emulsifier, styrene and an unsaturated monomer are mixed and stirred for emulsification to obtain a pre-emulsion; the remaining softened water, the remaining emulsifier, a portion of the pre-emulsion and a portion of a water-soluble initiator solution are subjected to a first temperature-raising reaction under a protective gas atmosphere; the temperature is continued to be raised, the remaining pre-emulsion is added dropwise, and the remaining water-soluble initiator solution is added in batches for a second temperature-raising reaction; after cooling, a silane prepolymer, an oil-soluble initiator solution and a reducing agent solution are added in sequence under stirring for a cooling reaction, and the organosilicon-modified acrylic emulsion is obtained after the pH is adjusted.

7. The preparation method according to claim 6, characterized in that: The water-soluble initiator solution is a solution prepared by dissolving the water-soluble initiator in the softened water. Preferably, the concentration of the water-soluble initiator solution is 4-6 wt %; and / or, The solvent of the oil-soluble initiator solution is isopropanol or propylene glycol methyl ether. Preferably, the concentration of the oil-soluble initiator solution is 40-60 wt %; and / or, The reducing agent solution is a solution prepared by dissolving the reducing agent in the softened water. Preferably, the concentration of the reducing agent solution is 4-6 wt %; and / or, The stirring emulsification time is 15-30 minutes, and / or the stirring speed is 800-1200 rpm; and / or, The reaction temperature of the first temperature-raising reaction is 72-78° C., and / or, the first temperature-raising reaction is performed until the reaction system turns blue; and / or, The time for dripping the remaining pre-emulsion is 1.5-2 hours, and / or the reaction temperature of the second temperature-raising reaction is 80-85° C., and / or the reaction time of the second temperature-raising reaction is 0.5-1 hour; and / or, The dropping time of the reducing agent solution is 0.5-1h, and / or the reaction temperature of the cooling reaction is 50-60°C, and / or the reaction time of the cooling reaction is 0.5-1 hour; and / or, The pH after adjustment is 7-8.

8. A water-based heat-insulating coating using the organosilicon-modified acrylic emulsion as claimed in any one of claims 1 to 5 or the organosilicon-modified acrylic emulsion prepared by the preparation method as claimed in claim 6 or 7, characterized in that The water-based thermal insulation coating is prepared from raw materials including the following components: Silicone-modified acrylic emulsion, film-forming aid, pigment, filler, hollow glass microsphere, additive, thickener and softened water; Each component is calculated by weight: 100 parts by weight of silicone-modified acrylic emulsion; 5-8 parts by weight of film-forming aid, preferably 6-7 parts by weight; Pigment 10-50 parts by weight, preferably 30-40 parts by weight; Filler 25-70 parts by weight, preferably 30-50 parts by weight; 30-60 parts by weight, preferably 40-50 parts by weight, of hollow glass microspheres; 2.5-10 parts by weight of auxiliary agent, preferably 3-6 parts by weight; Thickener 0.6-1.5 parts by weight, preferably 0.8-1.2 parts by weight; 50-80 parts by weight of demineralized water, preferably 60-70 parts by weight.

9. The water-based thermal insulation coating according to claim 8, characterized in that: The film-forming aid is at least one of dodecyl alcohol ester, hexadecanol ester, dipropylene glycol monobutyl ether, and tripropylene glycol monobutyl ether; and / or, The infrared absorption rate of the pigment is ≤50%, and / or the infrared reflectivity is ≥25%; preferably, the pigment is at least one of titanium dioxide, titanium nickel yellow, and iron oxide yellow; and / or, The filler is at least one of fine talc powder, heavy calcium carbonate, precipitated barium sulfate, silicon powder, and magnesium hydroxide; and / or, The hollow glass microspheres are non-porous hollow structures. Preferably, the particle size of the hollow glass microspheres is 20-120 μm, and / or the true density is 0.15-0.4 g / cm 3 and / or, The auxiliary agent is at least one of a dispersant, a wetting agent, a leveling agent, a defoaming agent, a mildew preventer, and a preservative; and / or, The softened water is deionized water or distilled water. Preferably, the conductivity of the softened water is ≤20 μs / cm.

10. A method for preparing a water-based thermal insulation coating as claimed in claim 8 or 9, characterized in that The method comprises: Softened water, additives, pigments, fillers and part of thickeners are mixed and ground to obtain a color paste, and the color paste, silicone-modified acrylic emulsion, film-forming additives, hollow glass microbeads and the remaining thickener are mixed, and the pH is adjusted and then filtered to obtain the water-based thermal insulation coating.

11. A water-based heat-reflective topcoat using the organosilicon-modified acrylic emulsion according to any one of claims 1 to 5 or the organosilicon-modified acrylic emulsion prepared by the preparation method according to claim 6 or 7, characterized in that The water-based heat-reflective topcoat is prepared from raw materials including the following components: Silicone-modified acrylic emulsion, film-forming aid, pigment, filler, hollow glass microsphere, covering polymer, heat-reflective titanium dioxide, additives, thickener and softened water; Each component is calculated by weight: 100 parts by weight of silicone-modified acrylic emulsion; 5-8 parts by weight, preferably 5-7 parts by weight, of a film-forming aid; Pigment 0-20 parts by weight, preferably 5-18 parts by weight; 10-40 parts by weight of filler, preferably 20-30 parts by weight; 10-20 parts by weight, preferably 10-15 parts by weight, of hollow glass microspheres; 10-20 parts by weight of covering polymer, preferably 12-18 parts by weight; 10-30 parts by weight of heat reflective titanium dioxide, preferably 15-25 parts by weight; 1-5 parts by weight of auxiliary agent, preferably 2-4 parts by weight; Thickener 0.4-1.0 parts by weight, preferably 0.6-0.8 parts by weight; 20-30 parts by weight of demineralized water, preferably 22-28 parts by weight.

12. The water-based heat-reflective topcoat according to claim 11, characterized in that: The film-forming aid is at least one of dodecyl alcohol ester, hexadecanol ester, dipropylene glycol monobutyl ether, and tripropylene glycol monobutyl ether; and / or, The infrared absorptivity of the pigment is ≤50%, and / or the infrared reflectivity is ≥25%; preferably, the pigment is at least one of iron oxide red, iron oxide yellow, titanium nickel yellow, cobalt blue, phthalocyanine blue, chromium oxide green, iron chrome black, and perylene black; and / or, The filler is at least one of fine talc powder, ultrafine calcium carbonate, precipitated barium sulfate, silicon powder, and magnesium hydroxide; and / or, The hollow glass microspheres are non-porous hollow structures. Preferably, the particle size of the hollow glass microspheres is 20-120 μm, and / or the true density is 0.15-0.4 g / cm 3 and / or, The covering polymer is a polymer emulsion containing polymer hollow microspheres; and / or, The heat-reflective titanium dioxide is a rod-shaped rutile titanium dioxide. Preferably, the heat-reflective titanium dioxide has a short diameter of 0.3-0.5 μm and / or a long diameter of 2-4 μm; and / or, The auxiliary agent is at least one of a dispersant, a wetting agent, a leveling agent, a defoaming agent, a mildew preventer, and a preservative; and / or, The softened water is deionized water or distilled water. Preferably, the conductivity of the softened water is ≤20 μs / cm.

13. A method for preparing a water-based heat-reflective topcoat as claimed in claim 11 or 12, characterized in that The method comprises: Softened water, additives, pigments, fillers, heat-reflective titanium dioxide and part of thickener are mixed and ground to obtain a color paste, and the color paste, silicone-modified acrylic emulsion, film-forming additives, covering polymers, hollow glass microbeads and the remaining thickener are mixed, and the pH is adjusted and then filtered to obtain the water-based heat-reflective topcoat.

Citation Information

Patent Citations

  • Thermal-insulation paint

    CN104693934A

  • Composite functional type heat insulating coating for building wall

    CN105038422A

Cited By

  • Water-based anti-icing resin and preparation method thereof

    CN120865488A

  • High-weather-resistance water-based polymer emulsion and preparation method thereof

    CN122277821A