Preparation method of high polymer material containing sulfur and silicon and high polymer material containing sulfur and silicon
By injecting the sulfur-degraded sulfur and dimethyldivinyl silane in anti-sulfurization reaction, sulfur-containing silicon polymer materials were prepared, which solved the resource occupation and environmental pollution of industrial waste, and provided high-performance materials for multiple fields.
Patent Information
- Application Number
- CN202411221421.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-02
AI Technical Summary
The stacking of industrial waste sulfur and dimethyldivinylsilane leads to land resource occupation and environmental pollution, and lacks effective resource utilization methods.
By mixing and heating the precipitated sulfur and dimethyldivinyl silane, the polymerization product is formed and cured and quenched, a sulfur-containing silicon polymer material is obtained, and the re-sulfurization method is used to achieve resource utilization.
It effectively improves the land occupation and environmental pollution problems of industrial waste, and provides high-performance materials for heavy metal adsorption, lithium-sulfur ion batteries and electronic devices.
Smart Images

Figure CN118930861A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a preparation method of a sulfur-containing silicon polymer material and the sulfur-containing silicon polymer material. Background Art
[0002] Sulfur is a common industrial waste, which mainly comes from the hydrodesulfurization process of waste gas in the petroleum industry. At present, the annual production of sulfur in the world exceeds 70 million tons. Although 90% of it is effectively utilized, the rest can only be stored on the surface for a long time, occupying a large area of land and may cause harm to the environment.
[0003] Dimethyldivinylsilane is an inevitable byproduct in the Wurtz process of producing silicone vinyl capping agents, which are important raw materials for the production of silicone rubber. 50-80 kg of dimethyldivinylsilane is produced during the production of each ton of capping agent. This byproduct currently has no industrial use, and most of it is stored all year round. Only a small part of it evaporates into the atmosphere or is used as fuel, which takes up a lot of land resources and harms the environment. The structure of dimethyldivinylsilane is very suitable for the production of polymer materials, but there is currently a lack of research on the application of dimethyldivinylsilane.
[0004] Therefore, how to realize the resource utilization of sulfur and dimethyldivinylsilane is crucial to solving the problems of land resource occupation and environmental pollution. Summary of the invention
[0005] In view of the above shortcomings of the prior art, the present invention provides a method for preparing a sulfur-containing silicon polymer material and a sulfur-containing silicon polymer material to improve the land resource occupation and environmental pollution problems caused by the stacking of industrial waste sulfur and dimethyldivinylsilane.
[0006] To achieve the above-mentioned object and other related objects, the present invention provides a method for preparing a sulfur-containing silicon polymer material, the preparation method comprising the following steps:
[0007] The precipitated sulfur and dimethyldivinylsilane are mixed and heated to react to obtain a polymer product;
[0008] Cooling and curing the polymerized product to obtain a cured product;
[0009] The solidified product is quenched to obtain a sulfur-containing silicon polymer material.
[0010] In one example of the present invention, precipitated sulfur and dimethyldivinylsilane are mixed and heated to react, including: mixing the dimethyldivinylsilane and the precipitated sulfur in a reaction container at a mass ratio of 1:(4-19), heating the reaction container to 160°C to 190°C, and reacting for 1 to 3 hours.
[0011] In one example of the present invention, a reflux device is connected to the reaction container.
[0012] In one example of the present invention, the polymer product is cured by cooling, including, after the heating reaction is completed, cooling the reaction container to 130° C. and continuing the reaction for 24 to 80 hours.
[0013] In one example of the present invention, the quenching treatment of the solidified product includes: placing the container containing the solidified product in liquid nitrogen for 5 to 10 minutes.
[0014] In one example of the present invention, after the solidified product is quenched, it also includes a standing treatment and a purification treatment. The standing treatment includes: after the solidified product is quenched, standing at room temperature for 1 to 24 hours to obtain a crude product. After the crude product is purified, a sulfur-containing silicon polymer material is obtained.
[0015] In one example of the present invention, the purification process includes: grinding the crude product and placing it into a centrifuge tube, adding carbon disulfide and vortex mixing 3 to 5 times, then centrifuging using a centrifuge and pouring out the supernatant; repeating the above steps 3 to 5 times, and then transferring to an oven for drying to obtain a reddish-brown film or powder sulfur-containing silicon polymer material.
[0016] In one example of the present invention, the purification process includes: grinding the crude product and loading it into a vacuum sublimator containing a condensation device, evacuating the gas in the vacuum sublimator to reduce the internal pressure to 20 to 50 Pa; passing condensed water into the vacuum sublimator, heating it to 150°C, and maintaining it for 6 to 24 hours; after taking out the sample, washing it with carbon disulfide for 3 to 5 times, transferring it to an oven for drying, and obtaining a viscous black sulfur-containing silicon polymer material that is stable at room temperature.
[0017] The present invention also provides a sulfur-containing silicon polymer material, which is prepared by any of the above-mentioned preparation methods.
[0018] In one example of the present invention, the sulfur-containing silicon polymer material includes a structural unit represented by formula (1) and / or formula (2):
[0019]
[0020] Wherein, R in formula (1) and formula (2) represents a sulfur atom; Represents a sulfur chain or ring.
[0021] The invention uses precipitated sulfur and dimethyldivinylsilane as raw materials and adopts a reverse vulcanization method to polymerize to prepare a sulfur-containing silicon polymer material; the sulfur-containing silicon polymer material obtained by reverse vulcanization polymerization can be used in multiple fields such as heavy metal adsorption, lithium-sulfur ion batteries, electronic devices, etc., and has good application prospects.
[0022] The preparation method of the present invention realizes the resource utilization of settled sulfur and dimethyldivinylsilane industrial waste, and can effectively improve the land occupation and environmental pollution problems caused by the storage of industrial waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 A flow chart of a method for preparing a sulfur-containing silicon polymer material according to an embodiment of the present invention;
[0025] Figure 2 This is the solid-state NMR carbon spectrum of the crude product of the sulfur-containing silicon polymer material in one embodiment of the present invention. DETAILED DESCRIPTION
[0026] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.
[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0028] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0029] As used herein, "plurality", "multiple", "multiple times", etc., unless otherwise specified, refer to a quantity greater than or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0030] Herein, "preferred", "better" and "more preferred" are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute a limitation on the scope of protection of the present invention. If multiple "preferred" items appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "preferred" item is independent.
[0031] Herein, “further”, “furthermore”, “particularly”, etc. are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present invention.
[0032] In this article, when it comes to numerical ranges, unless otherwise specified, the distribution of optional values within the numerical range is considered continuous and includes the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical range, as well as every value between the two numerical endpoints. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined.
[0033] Sulfur and dimethyldivinylsilane are common industrial wastes. If stored on the surface, they will not only occupy a large amount of land resources, but also cause harm to the environment. In 2013, Pyun et al. found in their research that sulfur can undergo polymerization with terminal dienes under high temperature conditions, namely the "reverse vulcanization" technology, which provides a new path for the resource utilization of sulfur and dimethyldivinylsilane.
[0034] See also Figure 1 The present invention provides a method for preparing a sulfur-containing silicon polymer material, the preparation method comprising the following steps:
[0035] S1, mixing the precipitated sulfur and dimethyldivinylsilane, heating and reacting to obtain a polymer product;
[0036] S2, cooling and curing the reaction product to obtain a cured product;
[0037] S3, quenching the solidified product to obtain a sulfur-containing silicon polymer material.
[0038] The precipitated sulfur used in step S1 is a type of sulfur. The molecular formula of the precipitated sulfur is S8, which has a ring structure. Dimethyldivinylsilane is a byproduct produced in the process of producing silicone vinyl capping agent. The structural formula of dimethyldivinylsilane is (H2C=CH)2Si(CH3)2, which contains two vinyl groups (-CH=CH2), each of which contains a carbon-carbon double bond, so dimethyldivinylsilane is an unsaturated silicone compound.
[0039] When the precipitated sulfur and dimethyl divinyl silane are mixed, the cyclic molecules of the precipitated sulfur (S8) will open under high temperature conditions to form active sulfur. These active sulfurs can react with the carbon-carbon double bonds in dimethyl divinyl silane to form sulfur-carbon bonds, thereby connecting the sulfur molecules and dimethyl divinyl silane molecules to form a polymer with a three-dimensional network structure. This polymer contains a high proportion of sulfur and has multiple sulfur bond dynamic cross-linking sites.
[0040] The specific process of step S1 includes: mixing dimethyldivinylsilane and precipitated sulfur in a reaction container at a mass ratio of 1:(4-19), heating the reaction container to 160° C. to 190° C., and reacting for 1 to 3 hours.
[0041] The reaction container in this step can be a conventional glass container in the art, such as a flask, which can be a sealed container or an open container. The reaction container is connected to a reflux device. During the reaction process, the reflux device can reduce the volatilization loss of the reactants by condensation reflux; it can also control the temperature of the reaction system by condensation reflux to avoid side reactions or decomposition caused by overheating.
[0042] Dimethyldivinylsilane and precipitated sulfur are weighed according to a set ratio and added to the reaction vessel. The set ratio can be any ratio in the range of 1: (4 to 19), such as 1: 4, 1: 10, 1: 15 or 1: 19, etc. Then, the reaction vessel containing the reaction raw materials is heated by a heating device to cause the dimethyldivinylsilane and the precipitated sulfur to undergo a reverse vulcanization polymerization reaction. Among them, the heating device is, for example, an oil bath pot, that is, the reaction vessel is heated to 160°C to 190°C by using an oil bath pot, and reacted at this temperature for 1 to 3 hours. Specifically, the reaction temperature can be 160°C, 170°C, 180°C or 190°C, etc.; the reaction time can be 1 hour, 2 hours or 3 hours, etc., and the reaction temperature and reaction time can be selected according to actual conditions.
[0043] Step S2 is a curing treatment. After the heating reaction of step S1 is completed, the temperature of the reaction container is reduced to 130°C. The cooling method can be natural cooling, that is, it is maintained in an oil bath pot, and naturally reduced to 130°C as the temperature of the oil bath decreases, and the reaction is continued at this temperature for 24 to 80 hours. Through the curing treatment, the reaction product in a molten state can be converted into a solid cured product, the thermal stability of the material is improved, and the performance can be maintained at a higher temperature. The time of the curing treatment can be selected from any value in the range of 24 to 80 hours, for example, 24 hours, 40 hours, 60 hours or 80 hours, etc.
[0044] Step S3 is a quenching treatment, in which the reaction container after the solidification treatment is placed in liquid nitrogen and kept for 5 to 10 minutes, for example, 5 minutes, 8 minutes or 10 minutes. The boiling point of liquid nitrogen is very low (-195.8°C). In this step, liquid nitrogen can be used to quickly cool the reaction system to an extremely low temperature and immediately stop the reaction to avoid excessive cross-linking or side reactions and prevent structural changes during the cooling process.
[0045] After the quenching treatment is completed, the system is stored at -20°C to obtain a reddish-brown gel-like sulfur-containing silicon polymer material.
[0046] Furthermore, after the quenching treatment is completed, it also includes a standing treatment and a purification treatment, wherein the standing treatment is to stand the solidified product after the quenching treatment at room temperature for 1 to 24 hours, for example, standing for 1 hour, 10 hours, 15 hours or 24 hours to obtain a crude product; then the crude product is crushed and ground and then subjected to a purification process to obtain a sulfur-containing silicon polymer material. The crude product is usually in a block shape due to the bonding of the polymer. If it is not refined, it is not conducive to the subsequent purification process. Therefore, after the standing treatment and before the purification treatment, the crude product is first crushed and ground to obtain a powdered crude product. There is no restriction on the particle size after crushing and grinding here, and it only needs to be processed according to the conventional crushing and grinding process. It should be noted that the smaller the particles of the crude product, the more conducive to the purification of the product.
[0047] The purification treatment methods in this application include but are not limited to centrifugation and sublimation. Different purification treatment methods will result in different physical forms of the sulfur-containing silicon polymer material.
[0048] In one embodiment, the purification treatment is performed by centrifugation. The specific process is as follows: the powdered crude product is placed in a centrifuge tube, such as a 50 mL centrifuge tube, an appropriate amount of carbon disulfide is added and vortexed for 3 to 5 times, each time for 15 to 20 seconds, and then centrifuged in a high-speed centrifuge, for example, at 5000xg (multiples of the earth's gravity acceleration) for 3 minutes, and the supernatant is discarded; the steps of adding carbon disulfide, vortexing and high-speed centrifugation are repeated 3 to 5 times, and then transferred to an oven for drying to obtain a reddish-brown film or powder sulfur-containing silicon polymer material. The drying method is, for example, drying in a vacuum oven at 50°C for 12 to 24 hours.
[0049] In another embodiment, the purification treatment is carried out by sublimation. Specifically, the powdered crude product is loaded into a vacuum sublimator connected to a condensing device, and the gas in the vacuum sublimator is evacuated to maintain the internal pressure at 20 to 50 Pa; condensed water is introduced into the vacuum sublimator, and it is heated to 150°C and maintained at this temperature for 6 to 24 hours. Then the sample is taken out and washed with carbon disulfide for 3 to 5 times. Transfer it to an oven for drying to obtain a viscous black sulfur-containing silicon polymer material that is stable at room temperature. The above drying method is, for example, drying in a vacuum oven at 50°C for 12 to 24 hours.
[0050] In other embodiments, the purification treatment can also be carried out by calcination. For example, under nitrogen protection, calcination is performed at 240° C. in a tube furnace for 6 hours. Then, the sample is taken out and washed with carbon disulfide for 3 times. After being transferred to an oven for drying, a viscous black sulfur-containing silicon polymer material that is stable at room temperature can be obtained.
[0051] The present invention also provides a sulfur-containing silicon polymer material, which is prepared by polymerization reaction using precipitated sulfur and dimethyl divinyl silane as raw materials through a reverse vulcanization method. The preparation process of the sulfur-containing silicon polymer material can refer to the preparation method described above in the present invention, which will not be described in detail here.
[0052] The sulfur-containing silicon polymer material of the present invention comprises structural units represented by formula (1) and / or formula (2):
[0053]
[0054] Wherein, R in formula (1) and formula (2) represents a sulfur atom, It indicates a sulfur chain or sulfur ring of indeterminate length. The length of the sulfur chain and sulfur ring can be obtained through test analysis. The structural formula of sulfur-containing silicon polymer materials can be tested and analyzed by solid-state nuclear magnetic resonance, elemental analysis, ICP-OES (inductively coupled plasma emission spectrometer), etc. The sulfur-rich silicon polymer obtained by desulfurization has outstanding advantages such as excellent mercury and heavy metal adsorption performance, stable lithium-sulfur battery material performance, good thermal insulation performance, optical properties with high reflectivity factor, excellent antibacterial properties, and self-healing or cyclic properties.
[0055] The technical scheme of the present invention is described in detail below through several specific examples and comparative examples. Unless otherwise specified, the raw materials and reagents used in the following examples are all commercially available products, or can be prepared by conventional methods in the art, and the instruments used in the examples are all commercially available.
[0056] Example 1
[0057] 4.5020 g of precipitated sulfur was added into a closed reaction container connected to a reflux device, and then 0.5016 g of dimethyldivinylsilane was added and mixed, and the reaction system was heated to 185°C by a heating device, and stirred for reaction at this temperature for 1 hour; then the temperature was lowered to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 24 hours; then the reaction container was taken out, quenched under liquid nitrogen for 5 minutes, and then the reaction container was stored at -20°C to obtain a reddish-brown gel sulfur-containing silicon polymer material.
[0058] Example 2
[0059] 4.5007g of precipitated sulfur was added to a closed reaction vessel connected to a reflux device, and then 0.5006g of dimethyldivinylsilane was added and mixed. The reaction system was heated to 185°C by a heating device, and stirred for reaction at this temperature for 1h; then the temperature was lowered to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 24h; then the reaction container was taken out, placed in liquid nitrogen for quenching for 8min, and then the reaction container was stored at -20°C to obtain a reddish brown gel containing sulfur and silicon polymer material.
[0060] Example 3
[0061] 4.0142 g of precipitated sulfur was added into a closed reaction container connected to a reflux device, and then 1.0105 g of dimethyldivinylsilane was added and mixed, and the reaction system was heated to 185°C by a heating device, and the reaction was stirred for 1.5 hours; then the temperature was lowered to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 45 hours; then the reaction container was taken out, placed in liquid nitrogen for quenching for 5 minutes, and then the reaction container was stored at -20°C to obtain a reddish-brown gel sulfur- and silicon-containing polymer material.
[0062] Example 4
[0063] 4.2548 g of precipitated sulfur was added into a closed reaction container connected to a reflux device, and then 0.7502 g of dimethyldivinylsilane was added and mixed, and the reaction system was heated to 190°C by a heating device, and stirred for reaction at this temperature for 2 hours; then the temperature was lowered to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 45 hours; then the reaction container was taken out, quenched under liquid nitrogen for 10 minutes, and then the reaction container was stored at -20°C to obtain a reddish-brown gel sulfur- and silicon-containing polymer material.
[0064] Example 5
[0065] 4.4963 g of precipitated sulfur was added into a closed reaction container connected to a reflux device, and then 0.4986 g of dimethyldivinylsilane was added and mixed, and the reaction system was heated to 160° C. using a heating device, and stirred for reaction at this temperature for 3 hours; then the temperature was lowered to 130° C. (the temperature of the heating device was adjusted to 130° C., and the reaction system was naturally cooled to 130° C.), and solidified at this temperature for 45 hours; then the reaction container was taken out, quenched in liquid nitrogen for 5 minutes, and then the reaction container was stored at -20° C. to obtain a reddish-brown gel-containing sulfur and silicon polymer material.
[0066] Example 6
[0067] 4.4979 g of precipitated sulfur was added into a closed reaction container connected to a reflux device, and then 0.5101 g of dimethyldivinylsilane was added and mixed, and the reaction system was heated to 175°C by a heating device, and stirred for reaction at this temperature for 1 hour; then the temperature was lowered to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 45 hours, and then the reaction container was taken out and quenched in liquid nitrogen for 5 minutes, and then the reaction container was stored at -20°C to obtain a reddish-brown gel sulfur- and silicon-containing polymer material.
[0068] Example 7
[0069] 4.5088 g of precipitated sulfur was added to a closed reaction container connected to a reflux device, and then 0.5097 g of dimethyldivinylsilane was added and mixed. The reaction system was heated to 185°C using a heating device, and the reaction was stirred at this temperature for 1 hour; then the temperature was lowered to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 45 hours, and then the reaction container was taken out and quenched in liquid nitrogen for 5 minutes, and then the system was stored at -20°C to obtain a reddish-brown gel sulfur- and silicon-containing polymer material.
[0070] Example 8
[0071] 4.7531g of precipitated sulfur was added to a closed reaction vessel connected to a reflux device, and then 0.2519g of dimethyl divinyl silane was added and mixed, and the reaction system was heated to 185°C by a heating device, and stirred for reaction at this temperature for 1h; then the temperature was reduced to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 45h; then the reaction vessel was taken out, quenched under liquid nitrogen for 5min, and then the reaction vessel was placed at room temperature for 24h to obtain a crude product. The crude product was crushed and ground into powder, and the powdered crude product was grouped into 50mL centrifuge tubes, 1g per group, 35mL of carbon disulfide was added and vortexed for 3 times, each time for 20 seconds, and then centrifuged at 5000xg for 3min using a high-speed centrifuge, and the supernatant was poured out. The steps of adding carbon disulfide to the centrifuge tube, vortex mixing, and centrifugation were repeated three times, and then the tube was transferred to a vacuum oven at 50° C. and dried for 24 hours to obtain a dark reddish-brown thin film polymer material.
[0072] Example 9
[0073] 4.5039g of precipitated sulfur was added to a closed reaction vessel connected to a reflux device, and then 0.5068g of dimethyl divinyl silane was added and mixed. The reaction system was heated to 185°C using a heating device, and stirred for reaction at this temperature for 1h; then the temperature was reduced to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 45h; then the reaction vessel was taken out, quenched under liquid nitrogen for 5min, and then the reaction vessel was placed at room temperature for 24h to obtain a crude product. The crude product was crushed and ground into powder, and the powder was packed into 50mL centrifuge tubes, 1g per group, 35mL of carbon disulfide was added and vortexed for 3 times, each time for 20 seconds, and then centrifuged at 5000xg for 3min using a high-speed centrifuge, and the supernatant was discarded. The steps of adding carbon disulfide to the centrifuge tube, vortex mixing, and centrifugation were repeated three times, and then the tube was transferred to a vacuum oven at 50° C. and dried for 24 hours to obtain a dark reddish-brown thin film polymer material.
[0074] Example 10
[0075] 4.5022g of precipitated sulfur was added to a closed reaction vessel connected to a reflux device, and then 0.5030g of dimethyl divinyl silane was added and mixed, and the reaction system was heated to 185°C by a heating device, and stirred for reaction at this temperature for 1h; then the temperature was reduced to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 65h; then the reaction vessel was taken out, quenched under liquid nitrogen for 5min, and then the reaction vessel was placed at room temperature for 24h to obtain a crude product. The crude product was crushed and ground into powder, and the powder was packed into 50mL centrifuge tubes, 1g per group, 35mL of carbon disulfide was added and vortexed for 3 times, each time for 20 seconds, and then centrifuged at 5000xg for 3min using a high-speed centrifuge, and the supernatant was discarded. The steps of adding carbon disulfide to the centrifuge tube, vortex mixing, and centrifugation were repeated three times, and then the tube was transferred to a vacuum oven at 50° C. and dried for 24 hours to obtain a dark reddish-brown thin film polymer material.
[0076] Embodiment 11
[0077] 4.5036g of precipitated sulfur was added to a closed reaction vessel connected to a reflux device, and then 0.5048g of dimethyl divinyl silane was added and mixed, and the reaction system was heated to 185°C by a heating device, and stirred for reaction at this temperature for 1h; then the temperature was reduced to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 65h, and then the reaction vessel was taken out and quenched under liquid nitrogen for 5min, and then the reaction vessel was placed at room temperature for 24h to obtain a crude product. The crude product was crushed and ground into powder, and the powder was packed into 50mL centrifuge tubes, 1g per group, 35mL of carbon disulfide was added and vortexed for 3 times, each time for 20 seconds, and then centrifuged at 5000xg for 3min using a high-speed centrifuge, and the supernatant was poured out. The steps of adding carbon disulfide to the centrifuge tube, vortex mixing, and centrifugation were repeated three times, and then the tube was transferred to a vacuum oven at 50° C. and dried for 24 hours to obtain a dark reddish brown solid polymer material.
[0078] Example 12
[0079] 4.4976g of precipitated sulfur was added to a closed reaction vessel connected to a reflux device, and then 0.5022g of dimethyl divinyl silane was added and mixed. The reaction system was heated to 185°C by a heating device, and stirred for reaction at this temperature for 1h; then the temperature was lowered to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 65h, and then the reaction vessel was taken out and placed at room temperature for 48h to obtain a crude product. The crude product was crushed and ground into powder, and the powdered crude product was grouped into 50mL centrifuge tubes, 1g per group, 35mL of carbon disulfide was added and vortexed for 3 times, each time for 20 seconds, and then centrifuged at 5000xg for 3min using a high-speed centrifuge, and the supernatant was discarded. Repeat the steps of adding carbon disulfide to the centrifuge tube, vortexing, and centrifuging 3 times, and then transferred to a vacuum oven at 50°C and dried for 24h to obtain a dark reddish brown solid polymer material.
[0080] Embodiment 13
[0081] 4.4976 g of precipitated sulfur was added to a closed reaction container connected to a reflux device, and then 0.5041 g of dimethyldivinylsilane was added and mixed. The reaction system was heated to 185°C using a heating device, and the reaction was stirred at this temperature for 1 hour; then the temperature was lowered to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 80 hours; then the reaction container was taken out, quenched under liquid nitrogen for 5 minutes, and then the reaction container was placed at room temperature for 24 hours to obtain a crude product. The crude product was crushed and ground into powder, and the powdered crude product was grouped into a 60 mL flat-bottom sublimator, 1 g per group. The inside of the sublimator was evacuated to reduce the air pressure to about 30 Pa, and then condensed water was introduced into the sublimator and heated to 150°C, and maintained at this temperature for 6 hours. The black viscous substance at the bottom of the sublimator was taken out, washed with carbon disulfide for 3 times, and then transferred to a vacuum oven at 50°C and continued to dry for 24 hours to obtain a black viscous sulfur- and silicon-containing polymer material.
[0082] Embodiment 14
[0083] 4.4982g of precipitated sulfur was added to a closed reaction vessel connected to a reflux device, and then 0.5011g of dimethyldivinylsilane was added and mixed, and the reaction system was heated to 185°C by a heating device, and stirred for reaction at this temperature for 1h; then the temperature was reduced to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 65h; then the reaction vessel was taken out, quenched under liquid nitrogen for 5min, and then the reaction vessel was placed at room temperature for 24h to obtain a crude product. The crude product was crushed and ground into powder, loaded into a glass boat, and then loaded into the glass tube of a tube furnace, nitrogen was introduced into it, and the tube furnace was heated to 240°C for 6 hours; the black viscous substance at the bottom of the glass boat was taken out, washed with carbon disulfide 3 times, and then transferred to a vacuum oven at 50°C and continued to dry for 24h to obtain a black viscous sulfur- and silicon-containing polymer material.
[0084] Embodiment 15
[0085] 4.4976 g of precipitated sulfur was added to a closed reaction container connected to a reflux device, and then 0.5041 g of dimethyldivinylsilane was added and mixed. The reaction system was heated to 185°C using a heating device, and the reaction was stirred at this temperature for 1 hour; then the temperature was lowered to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 65 hours; then the reaction container was taken out, quenched under liquid nitrogen for 5 minutes, and then the reaction container was placed at room temperature for 24 hours to obtain a crude product. The crude product was crushed and ground into powder, and the powdered crude product was grouped into a 60 mL flat-bottom sublimator, 1 g per group. The inside of the sublimator was evacuated to reduce the air pressure to about 30 Pa, and then condensed water was introduced into the sublimator and heated to 150°C, and maintained at this temperature for 24 hours. The black viscous substance at the bottom of the sublimator was taken out, washed with carbon disulfide for 3 times, and then transferred to a vacuum oven at 50°C and continued to dry for 24 hours to obtain a black viscous sulfur- and silicon-containing polymer material.
[0086] Example 16
[0087] 4.4969g of precipitated sulfur was added to a closed reaction vessel connected to a reflux device, and then 0.5083g of dimethyldivinylsilane was added and mixed. The reaction system was heated to 185°C by a heating device, and the reaction was stirred at this temperature for 1h; then the temperature was reduced to 130°C (the temperature of the heating device was adjusted to 130°C, and the reaction system was naturally cooled to 130°C), and solidified at this temperature for 45h; then the reactor was taken out, quenched, and then the system was placed at room temperature for 24h to prepare a crude product. The crude product was crushed and ground into powder, and the powder crude product was grouped into a 60mL flat-bottomed sublimator, 1g per group, and the inside of the sublimator was evacuated to reduce the air pressure to about 30Pa, and then the reaction container was taken out and placed under liquid nitrogen for quenching for 5min, and then the reaction container was placed at room temperature for 24h to obtain a crude product. The crude product was crushed and ground into powder, and the powdered crude product was grouped into a 60 mL flat-bottom sublimator, 1 g per group. The inside of the sublimator was evacuated to reduce the air pressure to about 30 Pa, and then condensed water was introduced into the sublimator and heated to 150°C, and maintained at this temperature for 24 hours. The black viscous substance at the bottom of the sublimator was taken out, washed with carbon disulfide for 3 times, and then transferred to a vacuum oven at 50°C and continued to dry for 24 hours to obtain a black viscous sulfur- and silicon-containing polymer material.
[0088] In Examples 1 to 7, no purification treatment was performed after quenching to obtain gel-like sulfur- and silicon-containing polymer materials. In Examples 8 to 12, impurities in the products were separated by purification treatment using centrifugal washing after quenching to obtain dark reddish-brown film-like or solid polymer materials. In Examples 13, 15 and 16, sublimation washing was performed after quenching, and in Example 14, tubular furnace calcination was used for purification. All of these methods heated the products, which may cause decomposition of certain heat-sensitive components or changes in the degree of polymerization, thereby obtaining black viscous sulfur- and silicon-containing polymer materials.
[0089] The polymer materials of Examples 1 to 16 are all prepared by using precipitated sulfur and dimethyldivinylsilane as raw materials and polymerization reaction using the reverse vulcanization technology. The reason why they show different physical colors is that the purification can remove the excess sulfur element in the reactants, and the physical purification and chemical purification affect their molecular state. The polymer materials prepared in Examples 1 to 16 contain structural units represented by formula (1) and / or formula (2), which can be tested and analyzed by solid nuclear magnetic resonance, elemental analysis, ICP-OES (inductively coupled plasma emission spectrometer), etc. The crushed crude product prepared according to the conditions in Example 9 was characterized by its solid nuclear magnetic carbon spectrum, and the data are as follows: Figure 2As shown, the carbon atom signals in different structures of the polymer material are marked in the figure, and the data can prove that the polymer material includes the structural units shown in formula (1) and / or formula (2). The polymer material can be applied to various fields such as lithium-sulfur batteries, molybdenum sulfide two-dimensional electronic devices, and replacing conventional asphalt, and has good application prospects.
[0090] The present invention uses sedimented sulfur and dimethyldivinylsilane as raw materials, and adopts a reverse vulcanization method to polymerize to obtain a sulfur-containing silicon polymer material; the sulfur-containing silicon polymer material obtained by reverse vulcanization polymerization can be used in multiple fields such as heavy metal adsorption, lithium sulfur ion batteries, electronic devices, etc., and has good application prospects. The present invention realizes the resource utilization of sedimented sulfur and dimethyldivinylsilane industrial waste, and can effectively improve the land occupation and environmental pollution problems caused by the storage of industrial waste. Therefore, the present invention effectively overcomes some practical problems in the prior art and has a high utilization value and use significance.
[0091] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing a sulfur-containing silicon polymer material, characterized in that: The following steps are involved: The precipitated sulfur and dimethyldivinylsilane are mixed and heated to react to obtain a polymer product; Cooling and curing the polymerized product to obtain a cured product; The solidified product is quenched to obtain a sulfur-containing silicon polymer material.
2. The preparation method according to claim 1, characterized in that: The precipitated sulfur and dimethyldivinylsilane are mixed and heated for reaction, comprising: mixing the dimethyldivinylsilane and the precipitated sulfur in a reaction container at a mass ratio of 1:(4-19), heating the reaction container to 160° C. to 190° C., and reacting for 1 to 3 hours.
3. The preparation method according to claim 2, characterized in that: The reaction container is connected with a reflux device.
4. The preparation method according to claim 1, characterized in that: The polymer product is cooled and solidified, comprising: after the heating reaction is completed, the reaction container is cooled to 130° C., and the reaction is continued for 24 to 80 hours.
5. The preparation method according to claim 1, characterized in that: The solidified product is quenched, comprising: placing a reaction container containing the solidified product in liquid nitrogen for 5 to 10 minutes.
6. The preparation method according to claim 1, characterized in that: After the solidified product is quenched, it also includes a standing treatment and a purification treatment. The standing treatment includes: after the solidified product is quenched, standing at room temperature for 1 to 24 hours to obtain a crude product. After the crude product is purified, a sulfur-containing silicon polymer material is obtained.
7. The preparation method according to claim 6, characterized in that: The purification process comprises: grinding the crude product and placing it into a centrifuge tube, adding carbon disulfide and vortex mixing for 3 to 5 times, centrifuging using a centrifuge, and pouring out the supernatant; repeating the above steps for 3 to 5 times, and then transferring to an oven for drying to obtain a reddish-brown film or powder sulfur-containing silicon polymer material.
8. The preparation method according to claim 6, characterized in that: The purification process comprises: grinding the crude product and loading it into a vacuum sublimator containing a condensing device, evacuating the gas in the vacuum sublimator to reduce the internal pressure to 20 to 50 Pa; introducing condensed water into the vacuum sublimator, heating it to 150° C., and maintaining it for 6 to 24 hours; taking out the sample, washing it with carbon disulfide for 3 to 5 times, transferring it to an oven for drying, and obtaining a viscous black sulfur-containing silicon polymer material that is stable at room temperature.
9. A sulfur-containing silicon polymer material, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 8.
10. The sulfur-containing silicon polymer material according to claim 9, characterized in that: The sulfur-containing silicon polymer material comprises a structural unit represented by formula (1) and / or formula (2): Wherein, R in formula (1) and formula (2) represents a sulfur atom; Represents a sulfur chain or ring.
Citation Information
Patent Citations
Process for preparing sulfur containing organosilane polymers
CN112437785A
Sulfur-containing organosilicon compound, and method for producing the same
JP2001226383A
Method for producing sulfur-modified silicon compound and method for producing silicon disulfide
JP2011162361A
Sulfur-based polymers
US20210324147A1
Bis-(silylethyl)-oligosulphides and process for their production
US4384132A