High-hardness PC alloy and preparation method thereof

By using a water-absorbing resin and a silane coupling agent in the extruder, the surface hardness and modulus of polycarbonate (PC resin) are improved, and the problem of increasing hardness and modulus in the prior art is solved. , while maintaining the original properties of the resin.

CN118930874AActive Publication Date: 2024-11-12WANHUA CHEMICAL (NINGBO) CO LTD

Patent Information

Application Number
CN202411207338.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The prior art cannot efficiently improve the surface hardness and modulus of polycarbonate (PC resin) through modification technology, and does not affect the original high gloss and toughness of the resin.

Method used

The water-absorbent resin and a silane coupling agent are added to the extruder, and PC resin with silane groups is prepared through polymerization and cross-linking reactions to improve its surface hardness and modulus.

Benefits of technology

The surface hardness and modulus of PC alloys have been significantly improved, the surface hardness has been increased from 2B to 2H-3H, and the modulus has been increased from 2100MPa to 2400MPa, while maintaining the mechanical and thermal properties of PC resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005019395160000021
    Figure BDA0005019395160000021
  • Figure BDA0005019395160000031
    Figure BDA0005019395160000031
  • Figure BDA0005019395160000041
    Figure BDA0005019395160000041
Patent Text Reader

Abstract

The invention provides a high-hardness PC alloy and a preparation method thereof. The preparation method comprises the following steps: feeding the PC resin and the water-containing water-absorbent resin from a main feed of an extruder; feeding a silane coupling agent from a side feed of the extruder; and extruding and granulating by using an extruder to obtain the PC alloy material. According to the method, PC is degraded through water-absorbent resin, a PC chain segment with carboxyl and hydroxyl is generated, then the water-absorbent resin participates in polymerization, and a PC-water-absorbent resin chain segment is obtained through polymerization; a silane coupling agent is added to the rear section of the extruder and reacts with-COOH at the tail end of a PC chain segment, and the PC resin with silane groups is prepared. The PC resin is high in water absorption capacity after being extruded due to introduction of water absorption groups and does not need to be dried, silane groups are migrated to the surface by utilizing water vapor evaporated at a high temperature in an injection molding process and are crosslinked on the surface, so that high-hardness PC is prepared, and the surface hardness and modulus of PC alloy are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polycarbonate, and in particular relates to a high-hardness PC alloy and a preparation method thereof. Background Art

[0002] Polycarbonate (PC) is a widely used engineering plastic. Because of its high gloss and mechanical strength, PC is used in the appearance of various products, including 3C, wall switches, lamps, etc. However, the surface hardness and modulus of PC resin are not high, and it is easy to be scratched and bumped during production, transportation, and use, forming surface defects. Therefore, research on high-hardness PC is very important. The pencil hardness of commercially available general-purpose polycarbonate is around 3B and the modulus is around 2200MPa. At present, the industry mainly uses spray painting to improve the surface hardness and introduces fillers to improve the modulus; the former has complex processes, serious pollution and high costs, and the latter will affect the original high gloss and toughness of PC.

[0003] CN201610227475.3 discloses a painted product coated with a paint composition for polycarbonate glazing, which provides a hard coating on the primer layer by spraying, thereby providing good wear resistance to the polycarbonate; CN115785642A discloses a low-temperature resistant high-modulus electromagnetic shielding material and a preparation method thereof, which provides conductivity and high modulus properties by adding 10-20% of carbon-based conductive fillers.

[0004] At present, it is not possible to effectively improve the surface hardness and modulus of PC resin at the same time through modification technology without affecting the original properties of the resin. Summary of the invention

[0005] In view of the deficiencies in the prior art, one of the purposes of the present invention is to provide a method for preparing a high-hardness PC alloy, which significantly improves the surface hardness and modulus of the PC alloy without affecting the original properties of the resin.

[0006] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme:

[0007] A method for preparing a high-hardness PC alloy material, the method comprising the following steps:

[0008] S1: PC resin and water-containing absorbent resin are fed into the main feeding port of the extruder;

[0009] S2: Add the silane coupling agent from the feeding port on the extruder side;

[0010] S3: Extruder extrudes and granulates to obtain PC alloy material.

[0011] The present invention first adds a water-absorbing resin to the front section of the extruder to degrade PC and generate PC segments with carboxyl and hydroxyl groups, and then the water-absorbing resin participates in polymerization to polymerize into PC-water-absorbing resin segments; a silane coupling agent is added to the back section of the extruder to react with the -COOH at the end of the PC segment to prepare a PC resin with a silane group. Due to the introduction of water-absorbing groups, the PC resin has a strong water absorption capacity after extrusion, and the water content is about several thousand ppm. No drying is required, and the water vapor evaporated at high temperature during the injection molding process is used to migrate the silane group to the surface, and cross-linking occurs on the surface to prepare a high-hardness PC, which significantly improves the surface hardness and modulus of the PC alloy.

[0012] Exemplarily, the preparation process undergoes the following reaction:

[0013]

[0014]

[0015] In one embodiment of the present invention, the PC resin in S1 is an aromatic polycarbonate, an aliphatic polycarbonate and / or an aliphatic polycarbonate, preferably bisphenol A polycarbonate, more preferably one or more of Wanhua Chemical 2070, 2100, 2150, 2220, 2350; preferably, the PC resin has a melt flow index MFR of 5-50 g / 10 min, preferably 10-30 g / 10 min, under the test conditions of 300°C and a load of 1.2 kg; preferably, the PC resin has a mass fraction of 86-98 parts, preferably 90-95 parts.

[0016] In one embodiment of the present invention, the water-absorbing resin described in S1 is an acidic water-absorbing resin and / or an alcoholic water-absorbing resin, preferably one or more of acrylic acid water-absorbing resin, methacrylic acid resin, and polyethylene glycol resin; preferably, the molecular weight of the water-absorbing resin is 3000-10000.

[0017] In one embodiment of the present invention, the water content of the water-absorbing resin in S1 is 1-20 wt%, preferably 10-15 wt%; preferably, the water-absorbing resin contains 2-10 parts by weight, preferably 5-10 parts by weight.

[0018] As is well known in the art, an antioxidant or other auxiliary agent may be added to S1. Preferably, the antioxidant is a combination of one or more of hindered phenols, benzofurans, acryl-modified phenols, and hydroxylamines; preferably, one or more of hindered phenols.

[0019] In one embodiment of the present invention, the siloxane coupling agent described in S2 is a silane coupling agent with an -NH2 group, preferably one or more of γ-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, and γ-aminoethylaminopropyltrimethoxysilane; preferably, the mass proportion of the silane coupling agent is 0.5-2 parts, preferably 1-1.5 parts.

[0020] In one embodiment of the present invention, the extrusion granulation temperature of the extruder in S3 is 250-300°C, and the screw speed is 300-800rpm.

[0021] Exemplarily, the temperature can be preferably set in sections from the feed port to the die head as follows: 250-260°C at the feed port, 280-300°C for sections one to four, and 250-280°C for sections five to seven.

[0022] Another object of the present invention is to provide a high hardness PC alloy material.

[0023] A high-hardness PC alloy material, the material is prepared by the above method, and the material is prepared from the following components in parts by weight:

[0024]

[0025] Another object of the present invention is to provide a use of a high-hardness PC alloy material.

[0026] A use of a high-hardness PC alloy material. The material is prepared by the above method, or is the above material. The material is used to prepare a high-hardness PC product with a surface pencil hardness of 2H-3H.

[0027] For example, when preparing high-hardness PC products, the injection molding machine barrel temperature is set to 300-320° C., the injection pressure is 60-80 Bar, the mold temperature is 120-130° C., and the holding time is 1-3 s.

[0028] Compared with the prior art, the solution of the present invention has the following technical advantages:

[0029] The surface hardness and modulus of PC alloy are significantly improved (surface hardness is increased from 2B to 2H-3H, and modulus is increased from 2100MPa to 2400MPa), achieving high hardness of PC products without affecting the original mechanical and thermal properties of PC resin. DETAILED DESCRIPTION

[0030] The present invention is further described below by means of specific examples. The examples described in the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.

[0031] In the embodiments and comparative examples, the sources of the main raw materials are shown in Table 1 below:

[0032] Table 1 Raw material source information

[0033]

[0034]

[0035] Unless otherwise specified, other raw materials and reagents were purchased from commercial sources.

[0036] The processing equipment used was: twin-screw extruder, KraussMaffei ZE28 x40D BD, with an aspect ratio of 40 and a screw diameter of 28 cm;

[0037] The performance test parameters and corresponding test methods of PC alloy are as follows:

[0038] Moisture content (%): GB / T 2918-1998 "Determination of moisture content of plastic particles" is used, and a moisture meter is used for testing;

[0039] Pencil hardness: GB 6739-86 "Coating Hardness Pencil Hardness Method" is adopted;

[0040] Flexural strength and modulus (MPa): ISO 178:2010 "Plastics - Determination of flexural properties", speed 2mm / min;

[0041] Impact strength (MPa): Tested according to ISO 180-2000 "Determination of Izod impact strength of plastics";

[0042] Heat Deformation Temperature (℃): Tested using ISO 75 / B "Plastic Heat Deformation Temperature Test Method", with a heating rate of 120℃ / h.

[0043] Example 1

[0044] The high hardness PC alloy is prepared by the following raw material formula:

[0045]

[0046]

[0047] The preparation method is:

[0048] a. Place the water-absorbing resin in an environment of 23°C and 95% humidity to absorb water for 30 minutes, with a water content of 10wt%;

[0049] b. Add PC resin, acrylic acid water-absorbing resin and antioxidant from the main feed of the extruder;

[0050] c. Add γ-aminopropyltriethoxysilane from the side feed;

[0051] d. Extrusion conditions: control the vacuum degree of the vacuum device of the twin-screw metering section to be less than 0.08MPa, the screw speed to be 500rpm, and the screw temperature from the feed port to the die to be set to 255, 290, 290, 290, 290, 265, 265, 265;

[0052] e. Cool the extruded material at 50° C. in the water tank of the extruder and pelletize to obtain PC alloy;

[0053] f. The alloy in e is processed into a high hardness PC alloy product by injection molding temperature of 300°C, injection pressure of 80 Bar, mold temperature of 120°C and holding pressure of 2s.

[0054] Example 2

[0055] The high hardness PC alloy is prepared by the following raw material formula:

[0056]

[0057] The preparation method is:

[0058] a. Place the water-absorbing resin in an environment of 23°C and 95% humidity to absorb water for 20 minutes, with a water content of 5%;

[0059] b. Add PC resin, polyethylene glycol resin and antioxidant from the main feed of the extruder;

[0060] c. Add γ-aminoethylaminopropyltrimethoxysilane from the side feed;

[0061] d. Extrusion conditions: control the vacuum degree of the vacuum device of the twin-screw metering section to be less than 0.08MPa, the screw speed to be 300rpm, and the screw temperature from the feed port to the die to be set to 250, 280, 280, 280, 280, 250, 250, 250;

[0062] e. Cool the extruded material at 80°C in the water tank of the extruder and pelletize it to obtain a high-hardness PC alloy;

[0063] f. The alloy in e is processed into a high hardness PC alloy product by injection molding temperature of 300°C, injection pressure of 80 Bar, mold temperature of 120°C and holding pressure of 2s.

[0064] Example 3

[0065] The high hardness PC alloy is prepared by the following raw material formula:

[0066]

[0067] The preparation method is:

[0068] a. Place the water-absorbing resin in an environment of 23°C and 95% humidity to absorb water for 50 minutes, with a water content of 15%;

[0069] b. Add PC resin, methacrylic resin and antioxidant from the main feed of the extruder;

[0070] c. Add γ-aminoethylaminopropyltrimethoxysilane from the side feed;

[0071] d. Extrusion conditions: control the vacuum degree of the vacuum device of the twin-screw metering section to be less than 0.08MPa, the screw speed to be 800rpm, and the screw temperature from the feed port to the die to be set in sections as: 260, 300, 300, 300, 300, 280, 280, 280;

[0072] e. Cool the extruded material at 30°C in the water tank of the extruder and pelletize it to obtain a high-hardness PC alloy;

[0073] F. The alloy in e is processed into a high hardness PC alloy product by injection molding temperature of 300°C, injection pressure of 80 Bar, mold temperature of 120°C and holding pressure of 2s.

[0074] Comparative Example 1

[0075] Compared with Example 1, the difference is that γ-aminopropyltriethoxysilane is not added.

[0076] Comparative Example 2

[0077] Compared with Example 1, the difference is that no water-absorbing resin is added.

[0078] Comparative Example 3

[0079] Compared with Example 1, the difference is that the water-absorbing resin does not contain water.

[0080] Comparative Example 4

[0081] Compared with Example 1, the difference is that all raw materials are added to the main feeding port.

[0082] The PC alloy materials obtained in Examples 1-3 (S1-S3) and Comparative Examples 1-4 (D1-D4) were evaluated by injection molding in an injection molding machine. The screw temperature was set to 260°C and the screw speed was set to 250 rpm. The samples after injection molding were subjected to performance testing. The relevant properties are shown in Table 2.

[0083] Table 2 Performance test results of products of Examples 1-3 (S1-S3) and Comparative Examples 1-4 (D1-D4)

[0084]

[0085]

[0086] It can be seen from Comparative Examples 1-4 and Examples 1-3 that the PC alloys in the Examples have higher surface hardness and bending modulus, and the mechanical properties and thermal properties of the PC alloys are well maintained. However, the comparative examples have disadvantages such as low surface hardness, low toughness, and reduced strength.

[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing high hardness PC alloy material, It is characterized in that The method comprises the following steps: S1: PC resin and water-containing absorbent resin are fed into the main feeding port of the extruder; S2: Add the silane coupling agent from the feeding port on the extruder side; S3: Extruder extrudes and granulates to obtain PC alloy material.

2. The method according to claim 1, It is characterized in that S1: The PC resin is aromatic polycarbonate and / or aliphatic polycarbonate, preferably bisphenol A polycarbonate, more preferably one or more of Wanhua Chemical 2070, 2100, 2150, 2220, and 2350; Preferably, the PC resin has a melt flow index MFR of 5-50 g / 10 min, preferably 10-30 g / 10 min, under the test conditions of 300° C. and a load of 1.2 kg.

3. The method according to claim 1 or 2, It is characterized in that The water-absorbing resin described in S1 is an acidic water-absorbing resin and / or an alcoholic water-absorbing resin, preferably one or more of an acrylic water-absorbing resin, a methacrylic resin, and a polyethylene glycol resin; Preferably, the molecular weight of the water-absorbing resin is 3000-10000; And / or, the water content of the water-absorbing resin in S1 is 1-20 wt %, preferably 10-15 wt %.

4. The method according to claim 1, It is characterized in that S2 The siloxane coupling agent is a siloxane coupling agent having -NH 2 The silane coupling agent of the group is preferably one or more of γ-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, and γ-aminoethylaminopropyltrimethoxysilane.

5. The method according to claim 1, It is characterized in that The extrusion granulation temperature of the extruder S3 is 250-300°C, and the screw speed is 300-800rpm.

6. A high-hardness PC alloy material, which is prepared by the method according to any one of claims 1 to 5. It is characterized in that The material is prepared from the following components in parts by weight:

7. Use of a high-hardness PC alloy material, wherein the material is prepared by the method according to any one of claims 1 to 5, or is the material according to claim 6, It is characterized in that The material is used for preparing high-hardness PC products with a surface pencil hardness of 2H-3H.

Citation Information

Patent Citations

  • PC-PA alloy material with outstanding heat resisting stability and preparation method thereof

    CN105176045A

  • Transparent flame retardant PC (Polycarbonate) material with high hardness and preparation method thereof

    CN105504751A

  • Water absorption master batch used for recycled material and preparation method thereof

    CN108329577A

  • Preparation method of PC alloy with low water absorption rate

    CN117565358A

  • Laminated resin sheet for molding, and molded article using same

    WO2022091810A1

Cited By

  • PC alloy with hardened surface through microwave curing and preparation method

    CN119752144A

  • Microwave-cured surface-hardened pc alloy and method of making

    CN119752144B