Polyimide flexible LED lamp strip circuit board film and preparation method thereof

By using bridge agent coating and modified ink layer in the polyimide flexible LED light strip circuit board film, the problems of yellowing and poor adhesion at high temperatures are solved, and high adhesion and high reflectivity are achieved. Suitable for the production of large-pack continuous circuit boards, improving product stability and efficiency.

CN118930936APending Publication Date: 2024-11-12FOSHAN AOBAI PACKAGING MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411174757.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing polyimide flexible LED light strip circuit board film is prone to yellowing at high temperatures, with high curing temperature and long curing time, resulting in poor adhesion, coating peeling and winding back, and product unstable.

Method used

Using a bridge agent coating, including epoxy resin and titanium dioxide, as the intermediate layer between the polyimide film substrate and the ink layer, the combination of anilox roller coating and micro-concave roller coating can achieve rapid curing and High adhesion and a white ink layer of modified acrylic resin and methyl etherified high imino melamine crosslinker are used to improve light reflectivity and corrosion resistance.

Benefits of technology

It realizes high adhesion, high temperature resistance, yellowing resistance, strong corrosion resistance and high reflectivity of polyimide flexible LED light strip circuit board film, which is suitable for the production of large-package continuous circuit boards, and improves the product Stability and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005010415220000071
    Figure BDA0005010415220000071
Patent Text Reader

Abstract

The invention discloses a polyimide flexible LED lamp strip circuit board film and a preparation method thereof, and the polyimide flexible LED lamp strip circuit board film comprises a polyimide film substrate, a bridging agent coating and an ink layer; the bridging agent coating is positioned between the polyimide film base material and the ink layer; the bridging agent coating comprises a bridging main agent and a bridging curing agent, and the bridging main agent comprises epoxy resin and titanium dioxide. The bonding between the polyimide film base material and the ink layer is realized through the bridging agent coating, and the bridging agent coating has good adhesive force to the polyimide film base material and the ink layer, so that the ink layer can be better attached to the polyimide film base material; therefore, the final polyimide flexible LED lamp strip circuit board film has the characteristics of high reflective rate, folding resistance, strong adhesive force, strong etching solution corrosion resistance, strong oxidation solution corrosion resistance, good temperature resistance, good yellowing resistance and the like, can meet the requirements of large-package continuous circuit boards, and is stable and efficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of flexible LED light strips, and in particular relates to a polyimide flexible LED light strip circuit board film and a preparation method thereof. Background Art

[0002] Flexible LED light strips are widely used in urban bright projects and lighting, which has led to the rapid growth of flexible LED circuit boards. The production of flexible LED circuit boards has also entered the roll-to-roll continuous long-line production mode from the original short board production (about 1 meter). Especially after the industry introduced the circular knife continuous production, higher requirements were put forward for the quality and production efficiency of polyimide (PI) cover film. Although PI film has high temperature resistance and good shrinkage resistance, it has poor adhesion to ordinary inks, and resins with good adhesion to PI film are often prone to high temperature yellowing, or high curing temperature and long curing time. Moreover, since the ink coated on the PI film generally requires a long curing time (10-15 minutes) and a high curing temperature (above 200°C), it is easy to cause insufficient curing, poor adhesion, coating shedding, and rewinding and sticking under normal coating construction, and the product is very unstable. Therefore, there are still many difficulties in applying ink on the polyimide flexible circuit board film to obtain high-quality flexible LED light strip circuit board film.

[0003] CN 107778979A discloses a PET and PI film universal insulating matte black electronic gravure ink and a preparation method thereof, specifically disclosing saturated polyester, modified polyurethane resin, hydroxy acrylic resin, 0.1-2 parts of dispersant; leveling agent, urea-formaldehyde resin modified matting powder, white carbon black, talcum powder, ultrafine kaolin, polyethylene wax, carbon black, n-propyl acetate, ethyl acetate, saturated polyester B, adhesion promoter and propylene glycol methyl ether acetate. This technical solution improves the adhesion of gravure ink on substrates such as PET and PI films by using resin components with different physical and chemical properties such as modified polyurethane resin and hydroxy acrylic resin, so that the gravure ink can be used on both PET and PI film substrates, but the problem of product instability in actual application needs to be further improved.

[0004] CN 116606565A discloses low-temperature curing insulating ink for PI membrane and its preparation method and construction process, and specifically discloses that the ink contains the following raw materials in weight percentage: 5-35% polyurethane resin, 10-60% solvent, 0.01-1% coupling agent, 0.01-5% defoamer, 0.01-5% leveling agent, 0-45% filler and 1-10% pigment. The low-temperature curing insulating ink for PI membrane of the technical solution has good fluidity and good printing performance. However, although the technical solution has made a good improvement on the ink, the overall product structure has not changed much and is still insufficient.

[0005] In summary, the prior art still requires a mature and reliable polyimide flexible LED light strip circuit board film preparation process. Summary of the invention

[0006] One of the purposes of the present invention is to provide a polyimide flexible LED light strip circuit board film, in which the bonding between the polyimide film substrate and the ink layer is achieved through a bridging agent coating, and the bridging agent coating has good adhesion to both the polyimide film substrate and the ink layer, so that the ink layer can be better adhered to the polyimide film substrate, thereby making the final polyimide flexible LED light strip circuit board film have the characteristics of high reflectivity, folding resistance, strong adhesion, strong resistance to etching liquid and anti-oxidation liquid corrosion, good temperature resistance, good yellowing resistance, etc., and at the same time, it can also meet the requirements of large-volume continuous circuit boards, which is both stable and efficient.

[0007] In order to achieve the above purpose, this application adopts the following technical solutions:

[0008] A polyimide flexible LED light strip circuit board film, comprising a polyimide film substrate, a bridging agent coating and an ink layer; the bridging agent coating is located between the polyimide film substrate and the ink layer;

[0009] The bridging agent coating comprises a bridging main agent and a bridging curing agent, and the bridging main agent comprises epoxy resin and titanium dioxide.

[0010] Furthermore, the epoxy resin is epoxy polyester resin; and the bridging curing agent is diphenylmethane diisocyanate.

[0011] Furthermore, the weight ratio of the bridging main agent to the bridging curing agent is 5:1; the weight ratio of the epoxy polyester resin and titanium dioxide in the bridging main agent is 2-3:1.

[0012] Furthermore, the bridging agent coating layer also includes matting powder, and the weight ratio of the matting powder in the bridging agent coating layer is 1-2%.

[0013] Furthermore, the ink layer includes an ink main agent and an ink curing agent, wherein the ink main agent includes a modified acrylic resin and titanium dioxide, and the ink curing agent includes a methyl etherified high-imino melamine cross-linking agent dissolved in isobutyl alcohol.

[0014] Furthermore, the weight ratio of the ink main agent to the ink curing agent is 7:3; the weight ratio of the modified acrylic resin and titanium dioxide in the ink main agent is 2-3:1.

[0015] The second object of the present application is to provide a method for preparing a polyimide flexible LED light strip circuit board film, comprising:

[0016] S1: coating a bridging agent coating on a polyimide film substrate and drying the coating to obtain a bridging agent coating comprising an epoxy resin and a bridging curing agent component;

[0017] S2: coating an ink layer on the coating bridging agent layer and drying the layer to obtain a polyimide flexible LED light strip circuit board film.

[0018] Furthermore, in step S1, the coating amount of the bridging agent coating is 2-3 g / m2, the drying temperature of the bridging agent coating is 180-190° C., and the drying time of the bridging agent coating is 40-50 seconds.

[0019] Furthermore, in step S2, the coating amount of the ink layer is 18-22 g / m2, the drying temperature of the bridging agent coating is 180-190° C., and the coating speed of the bridging agent coating is 30 m / min.

[0020] Furthermore, in step S1, the bridging agent coating layer is coated by anilox roller coating, and in step S2, the ink layer is coated by micro-concave roller coating.

[0021] The beneficial effects of the present invention are:

[0022] In the present application, the polyimide film serves as the main body of the flexible circuit board and plays the role of a substrate carrier. In the subsequent processing steps, it carries various functional coatings and composite materials and maintains the stiffness and flatness of the material. Even if it is cut into thin strips, the film roll can still be rolled up intact and straight, and it has considerable resistance to bending and pulling.

[0023] In the present application, the bridging agent coating plays a bridging role between the polyimide film substrate and the ink layer, so that a stable adhesion is formed between the polyimide film substrate and the ink layer, so that the physical properties of the overall coating, such as corrosion resistance, solvent resistance, folding resistance and temperature resistance, are stabilized at a high level; in view of the fact that the bridging agent coating has good adsorption to both the polyimide film substrate and the ink layer, the bridging agent coating can reduce the stringent requirements for the ink layer, making the selectivity of the ink layer more extensive. At the same time, since the polyimide film substrate and the bridging agent coating are covered by the ink layer, there are not too many requirements for the color measurement of the two. The polyimide film substrate itself is brown-yellow, and the bridging agent coating can allow an appropriate amount of yellow, and only needs to focus on its adhesion to the polyimide film substrate and the ink layer.

[0024] In this application, the ink layer is used for appearance decoration and external protection. White ink can be selected to make the polyimide flexible LED light strip circuit board film have high reflectivity and folding resistance, kneading resistance, corrosion resistance and other effects. At the same time, the white ink layer can cover the yellow hue of polyimide, improve the bright and high-end texture of white, and the reflectivity can be as high as 83% or more, meeting the reflective needs of circuit board production light strips; making the polyimide flexible LED light strip circuit board film have good high temperature shrinkage resistance, tensile strength, flame retardant performance and other properties. DETAILED DESCRIPTION

[0025] The specific implementation of the present invention is further described below in conjunction with specific embodiments:

[0026] With the widespread use of flexible LED light strips, higher requirements are placed on the quality and production efficiency of PI covering films: The specific requirements for the white coating of PI covering films are as follows: 1. Reflectivity of more than 83%; 2. High temperature resistance, resistance to flux (solder resist); 3. Good adhesion; 4. Resistance to high temperature yellowing; 5. Resistance to UV yellowing; 6. Resistance to bending; 7. For copper-clad etched boards, they must be resistant to etching liquids and acids and alkalis.

[0027] Although the PI film in the prior art has high temperature resistance and good shrinkage resistance, it has poor adhesion to ordinary inks, and resins with good adhesion to PI films are often prone to yellowing at high temperatures, or have high curing temperatures and long curing times. In view of the use scenarios of flexible LED light strips, yellow ink cannot be used, which will affect the reflectivity of the flexible LED light strips.

[0028] In order to solve the above problems, the present application provides a polyimide flexible LED light strip circuit board film, including a polyimide film substrate, a bridging agent coating and an ink layer; the bridging agent coating is located between the polyimide film substrate and the ink layer; the bridging agent coating includes a bridging main agent and a bridging curing agent, and the bridging main agent includes epoxy resin and titanium dioxide.

[0029] On the polyimide (PI) film substrate, a layer of bridging agent coating with a thickness of about 0.5-1 micron is first made by anilox roller coating with two-component varnish of epoxy resin and bridging curing agent, and then cured by baking at 180-190℃. The bridging agent coating focuses on ensuring the adhesion to the polyimide film substrate, and plays a role in the adhesion between the polyimide film substrate and the ink layer; because the amino resin system and polyurethane system resin formula have unsatisfactory adhesion to the polyimide (PI) film, only the isocyanate-cured flexible epoxy resin formula can have excellent adhesion, and the isocyanate-cured epoxy system coating has a slow reaction speed, and it is not easy to completely cure within the curing time of 20-30 seconds on the coating line, which often causes the problem of reverse sticking to the back of the roll. At the same time, the isocyanate-cured epoxy system coating also has defects in high temperature yellowing resistance, so it is suitable as a bridging agent coating and the thin coating should be controlled as much as possible to reduce the risk of back adhesion.

[0030] Specifically, the epoxy resin in the present application is epoxy polyester resin; the bridging curing agent is diphenylmethane diisocyanate. The weight ratio of the bridging main agent to the bridging curing agent is 5:1; the weight ratio of the epoxy polyester resin to titanium dioxide in the bridging main agent is 2-3:1. At the same time, the bridging agent coating also includes matting powder, and the weight ratio of the matting powder in the bridging agent coating is 1-2%.

[0031] This specific bridging agent coating formula has excellent adhesion to polyimide film, and because of its high cross-linking density and rich reactive groups, it is also very resistant to yellowing, high temperature and corrosion when cured. However, its disadvantage is that the complete reaction requires high temperature and a long reaction time. Usually, it takes more than 5 minutes at 180-190°C to complete the curing. The actual conditions for the high-speed coating method we use for drying and curing are only a short time of 40-50 seconds in an oven at 180-190°C. Therefore, this bridging layer cannot be applied too thickly, and the dry coating amount should be controlled below 2-3 grams / square meter. At the same time, 1-2% matting powder should be added as appropriate to prevent re-sticking due to low degree of curing.

[0032] After the bridging agent coating is formed, a white ink layer prepared by thermosetting acrylic resin, amino resin, elastic polyester resin and titanium dioxide is applied on the bridging agent coating by micro-concave roller coating. Depending on the reflectivity and hiding power, the thickness of the white coating needs to be adjusted to 20-35 microns, and it is baked and cured at a baking temperature of 190°C. This makes the white coating resistant to high temperatures, solvents, acids and alkalis, corrosion by oxidizing liquids, scratches, yellowing, folding, and suitable for printing.

[0033] Specifically, the ink layer includes an ink main agent and an ink curing agent, wherein the ink main agent includes a modified acrylic resin and titanium dioxide, and the ink curing agent includes a methyl etherified high-imino melamine crosslinking agent dissolved in isobutyl alcohol. The weight ratio of the ink main agent to the ink curing agent is 7:3; the weight ratio of the modified acrylic resin to the titanium dioxide in the ink main agent is 2-3:1.

[0034] The modified acrylic resin selected in the present application is specifically a low-temperature self-crosslinking thermoplastic low-hydroxyl value modified acrylic resin, which has the characteristics of heat resistance and yellowing resistance, fast drying and high reaction activity. Specifically, the low-temperature self-crosslinking thermoplastic low-hydroxyl value modified acrylic resin of brand JY-2243 can be selected, with a TG point of 40°C, an acid value of 20, a hydroxyl value of 30, and a dehydration reaction self-crosslinking temperature of 80°C.

[0035] The ink layer is a white ink layer. The white ink layer under the above specific formula has high activity, fast drying speed, good self-leveling and brightness. The final coating performance has excellent gloss, yellowing resistance, temperature resistance, acid and alkali corrosion resistance, flexibility, and printability. Since the overall coating requires considerable hiding power, the top coating is applied by anilox roller with a dry coating amount controlled at 18-22 g / m2, a curing temperature of 180-190°C, and a coating speed of 30 m / min.

[0036] The existing LED light strip circuit board film is coated with screen printing during the preparation process, which requires printing screen by screen, with low efficiency and high energy consumption. In addition, it is produced by coating with a coating machine. Since the ink coated with the PI film generally requires a long curing time (10-15 minutes) and a high curing temperature (above 200°C), it is easy to cause insufficient curing, poor adhesion, coating shedding, and re-sticking when rolled up under normal coating construction, and the product is very unstable.

[0037] In order to solve the above problems, the present application provides a method for preparing a polyimide flexible LED light strip circuit board film, comprising:

[0038] S1: coating a bridging agent coating on a polyimide film substrate and then drying the coating to obtain a bridging agent coating comprising epoxy resin and a bridging curing agent component.

[0039] Among them, a 25μ thick polyimide film is selected as the base material. The polyimide film is more resistant to high temperatures than the PET film, and has good insulation and acid and alkali corrosion resistance. In the subsequent processing steps, it carries various functional coatings and composite materials and maintains the stiffness and flatness of the material. Even if it is cut into thin strips, the film roll can still be rolled up intact and straight, and it has considerable resistance to bending and pulling.

[0040] A bridging agent coating is applied on a polyimide film substrate by an anilox roller coating method, the thickness of the bridging agent coating is about 0.5-1 micron, and the coating is quickly dried and cured at 180-190°C. The bridging agent coating includes a bridging main agent and a bridging curing agent, and the weight ratio of the bridging main agent to the bridging curing agent is 5:1; the weight ratio of the epoxy polyester resin and the titanium dioxide in the bridging main agent is 2-3:1. At the same time, the bridging agent coating also includes a matting powder, and the weight ratio of the matting powder in the bridging agent coating is 1-2%.

[0041] The bridging agent coating formula of the present application has excellent adhesion to the polyimide film, and because of its high crosslinking density and rich reactive groups, it is also very resistant to yellowing, high temperature and corrosion when cured. At the same time, since the thickness of the bridging agent coating is very thin and the coating amount is small, the dry coating amount is controlled below 2-3 grams per square meter. After coating by high-speed coating, it only needs to be dried in an oven at 180-190°C for 40-50 seconds to achieve drying and curing. At the same time, the 1-2% matting powder added to the bridging agent coating can avoid the re-sticking of the winding caused by the low degree of rapid curing of the bridging agent coating.

[0042] S2: coating an ink layer on the coating bridging agent layer and drying the layer to obtain a polyimide flexible LED light strip circuit board film.

[0043] In this step, the ink layer is coated by a micro-concave roller coating method after coating the bridging agent coating. The ink layer can be a white ink layer. The white ink layer includes an ink main agent and an ink curing agent. The ink main agent includes a modified acrylic resin and titanium dioxide. The ink curing agent includes a methyl etherified high-imino melamine cross-linking agent dissolved in isobutyl alcohol. The weight ratio of the ink main agent to the ink curing agent is 7:3; the weight ratio of the modified acrylic resin and titanium dioxide in the ink main agent is 2-3:1.

[0044] The coating amount of the ink layer is 18-22 g / m2, the drying temperature of the bridging agent coating is 180-190° C., and the coating speed of the bridging agent coating is 30 m / min.

[0045] S3: After coating, the finished product needs to be placed in a 60°C curing room for more than 72 hours to mature. After the curing is completed, epoxy resin glue can be used to glue the PI surface to form back protection for the polyimide film substrate.

[0046] The white coating surface layer of this application is resistant to solder paste flux (solder resist), high temperature baking, solvent resistance, yellowing resistance, acid and alkali resistance, and anti-oxidant corrosion. In addition to being used as a double-sided panel mask, it can also be used as an etching plate. The ink layer of this application can cover the yellow hue of polyimide, improve the bright and high-end texture of white, and the reflectivity can be as high as 83% or more, meeting the reflective needs of circuit board production light strips; PI film material is much higher than PET material products in terms of high temperature shrinkage resistance, tensile strength, flame retardancy and other important indicators.

[0047] The micro-concave coating method of this application is both efficient and stable, and is faster and more advanced than the process of white solder mask oil for screen printing.

[0048] Example 1

[0049] The present embodiment provides a polyimide flexible LED light strip circuit board film provided by the present application, comprising a polyimide film substrate, a bridging agent coating and an ink layer; the bridging agent coating is located between the polyimide film substrate and the ink layer; the bridging agent coating comprises a bridging main agent, a bridging curing agent and a matting powder, the bridging main agent comprises epoxy polyester resin and titanium dioxide; the bridging curing agent comprises diphenylmethane diisocyanate. The weight ratio of the bridging main agent and the bridging curing agent is 5:1; the weight ratio of the epoxy polyester resin and the titanium dioxide in the bridging main agent is 2.5:1; the weight ratio of the matting powder in the bridging agent coating is 1.5%.

[0050] The ink layer is a white ink layer, and the ink layer includes an ink main agent and an ink curing agent, wherein the ink main agent includes a modified acrylic resin and titanium dioxide, and the ink curing agent includes a methyl etherified high-imino melamine crosslinking agent dissolved in isobutyl alcohol. The weight ratio of the ink main agent to the ink curing agent is 7:3; the weight ratio of the modified acrylic resin to the titanium dioxide in the ink main agent is 2.5:1.

[0051] This embodiment also provides a method for preparing a polyimide flexible LED light strip circuit board film, comprising:

[0052] S1: A polyimide film with a thickness of 25 μ is selected as a substrate, a bridging agent coating is applied on the polyimide film substrate by an anilox roller coating method, and the coating is dried to obtain a bridging agent coating comprising epoxy resin and a bridging curing agent component.

[0053] The thickness of the bridging agent coating is about 0.5-1 micron, and the dry coating amount is controlled below 2-3 g / m2. After coating by high-speed coating, it only needs to be dried in an oven at 180-190°C for 40-50 seconds to achieve drying and curing. At the same time, the matting powder added to the bridging agent coating can avoid the re-sticking caused by the low degree of rapid curing of the bridging agent coating.

[0054] S2: coating an ink layer on the coating bridging agent coating layer by a micro-concave roller coating method, and drying the layer to obtain a polyimide flexible LED light strip circuit board film.

[0055] The ink layer formula in this embodiment has high activity, fast drying, good self-leveling and brightness. The final coating has excellent gloss, yellowing resistance, temperature resistance, acid and alkali corrosion resistance, flexibility, and printability. Since the overall coating requires considerable hiding power, the ink layer is coated with an anilox roller with a dry coating amount controlled at 18-22 g / m2, a curing temperature of 180-190°C, and a coating speed of 30 m / min.

[0056] S3: After coating, the finished product needs to be placed in a 60°C curing room for more than 72 hours to mature. After the curing is completed, epoxy resin glue can be used to glue the PI surface to form back protection for the polyimide film substrate.

[0057] The polyimide flexible LED light strip circuit board film prepared in this embodiment is tested by the testing method shown in Table 1. The specific testing items and achievement indicators are shown in Table 1.

[0058] Table 1 Detection method and index of polyimide flexible LED light strip circuit board film in Example 1

[0059]

[0060] From Table 1, it can be seen that the polyimide flexible LED light strip circuit board film prepared in this application has good adhesion, reflectivity, surface gloss, high temperature yellowing resistance, high temperature resistance, corrosion resistance, weather resistance and yellowing resistance, as well as good printability. Application scenarios In addition to being a double-sided panel mask, it can also be used as an etching plate.

[0061] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs may also make changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some modifications and changes to the invention should also fall within the scope of protection of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.

Claims

1. A polyimide flexible LED light strip circuit board film, characterized in that: It comprises a polyimide film substrate, a bridging agent coating and an ink layer; the bridging agent coating is located between the polyimide film substrate and the ink layer; The bridging agent coating comprises a bridging main agent and a bridging curing agent, and the bridging main agent comprises epoxy resin and titanium dioxide.

2. A polyimide flexible LED light strip circuit board film according to claim 1, characterized in that: The epoxy resin is epoxy polyester resin; the bridging curing agent is diphenylmethane diisocyanate.

3. A polyimide flexible LED light strip circuit board film according to claim 2, characterized in that: The weight ratio of the bridging main agent to the bridging curing agent is 5:1; the weight ratio of the epoxy polyester resin and titanium dioxide in the bridging main agent is 2-3:

1.

4. The polyimide flexible LED light strip circuit board film according to claim 1, characterized in that: The bridging agent coating layer further comprises matting powder, and the weight ratio of the matting powder in the bridging agent coating layer is 1-2%.

5. The polyimide flexible LED light strip circuit board film according to claim 1, characterized in that: The ink layer comprises an ink main agent and an ink curing agent, wherein the ink main agent comprises a modified acrylic resin and titanium dioxide, and the ink curing agent comprises a methyl etherified high-imino melamine cross-linking agent dissolved in isobutyl alcohol.

6. A polyimide flexible LED light strip circuit board film according to claim 5, characterized in that: The weight ratio of the ink main agent to the ink curing agent is 7:3; the weight ratio of the modified acrylic resin and titanium dioxide in the ink main agent is 2-3:

1.

7. A method for preparing a polyimide flexible LED light strip circuit board film, characterized in that: include: S1: coating a bridging agent coating on a polyimide film substrate and drying the coating to obtain a bridging agent coating comprising an epoxy resin and a bridging curing agent component; S2: coating an ink layer on the coating bridging agent layer and drying the layer to obtain a polyimide flexible LED light strip circuit board film.

8. The preparation method according to claim 7, characterized in that: In step S1, the coating amount of the bridging agent coating is 2-3 g / m2, the drying temperature of the bridging agent coating is 180-190° C., and the drying time of the bridging agent coating is 40-50 seconds.

9. The preparation method according to claim 7, characterized in that: In step S2, the coating amount of the ink layer is 18-22 g / m2, the drying temperature of the bridging agent coating is 180-190° C., and the coating speed of the bridging agent coating is 30 m / min.

10. The preparation method according to claim 7, characterized in that: In step S1, the bridging agent coating layer is coated by anilox roller coating, and in step S2, the ink layer is coated by micro-concave roller coating.