Preparation method and application of nano SiO2 / TiO2 coating modified BOPP (Biaxially-oriented Polypropylene) film

By preparing nano SiO2@TiO2 coating on BOPP film, BOPP/SiO2@TiO2 nanocomposite film was formed, and the adhesion of BOPP film in aqueous ink was solved using corona and ultraviolet graft polymerization technology and combined with screen printing technology. The problem of low printing quality has significantly improved adhesion and printing effect.

CN118930941APending Publication Date: 2024-11-12ZHEJIANG KINLEAD PACKAGING MATERIAL
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411013585.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

BOPP films have shortcomings in adhesion and printing quality of water-based inks, and few prior art have been reported.

Method used

The preparation method of modified BOPP film using nano SiO2@TiO2 coating, including corona pretreatment, ultraviolet graft polymerization and silicon titanium sol scraping, to form BOPP/SiO2@TiO2 nanocomposite film, and improve water properties through screen printing process Adhesion and printing quality of ink.

Benefits of technology

It significantly improves the wetting and bonding power of water-based inks, improves printing accuracy and adhesion, and solves the shortcomings of BOPP film in water-based ink screen printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930941A_ABST
    Figure CN118930941A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a nano SiO2 / TiO2 coating modified BOPP film. The preparation method mainly comprises the following steps: (1) cleaning and drying a BOPP film, and then carrying out corona treatment to obtain a BOPP corona film; (2) preparing a pre-polymerization solution, dispensing the pre-polymerization solution on a BOPP corona film, irradiating under an LED ultraviolet curing lamp for graft polymerization, after the reaction is finished, soaking with deionized water, washing with ethanol, and drying to obtain a BOPP / PAA grafted film; and (3) preparing a silicon-titanium sol with a certain concentration, and blade-coating the silicon-titanium sol on the BOPP / PAA grafted film. And reacting at room temperature, performing ultrasonic cleaning, and drying to obtain the nano SiO2 / TiO2 coating modified BOPP composite film. The invention also provides an application of the nano SiO2 / TiO2 coating modified BOPP film in water-based ink printing. Compared with other BOPP films, the printing precision and the adhesion performance of the water-based ink on the nano composite film are remarkably improved. The preparation method provided by the invention is simple, not only develops a novel nano coating modified BOPP film, but also solves the problem of poor printing effect of traditional BOPP film water-based ink.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of plastic films and specifically discloses a method for preparing a nano-SiO2@TiO2 coating modified BOPP film. Background Art

[0002] BOPP film is a film made of biaxially oriented polypropylene. It is widely used in food packaging, electronic product packaging, printing and other fields due to its excellent transparency, glossiness, moisture resistance, barrier properties and mechanical properties. However, as people's requirements for packaging continue to increase, higher requirements are also placed on the performance of BOPP film.

[0003] Corona is a widely used surface pretreatment method. After corona treatment, BOPP film can increase the surface tension of the material. Compared with corona pretreatment, the preparation of functional nano coating is another important way to modify the surface of BOPP film. Through the combination of organic and inorganic, a functional BOPP composite film can be developed that has both the easy processing and optical properties of BOPP film and the barrier and corrosion resistance of inorganic materials. For example, patent CN109897283A discloses a scratch-resistant BOPP film and a preparation method thereof. The scratch-resistant coating is formed by applying an anti-scratch coating containing nano-SiO2 on the surface of a BOPP corona film substrate and curing it with ultraviolet light. Min et al. found that coating a layer of SiO2 on a BOPP film can significantly increase the injection barrier, reduce charge injection, and thus reduce conductivity and Joule heat. Although the above studies show that BOPP film can be modified by nano-composite functions, there are few reports on water-based ink printing research.

[0004] Therefore, in view of the common problems of BOPP film such as low adhesion of water-based ink and low printing quality, the present invention proposes a nano-SiO2@TiO2 coating modified BOPP film and a preparation method thereof, which provides the possibility for the printing production of water-based ink for packaging, labels, etc. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a nano-SiO2@TiO2 coating modified BOPP film. To achieve the above purpose, the method specifically comprises the following steps:

[0006] (1) The BOPP film is ultrasonically cleaned with deionized water and ethanol in sequence, dried, and then corona pretreated to obtain a BOPP corona film;

[0007] (2) preparing a prepolymer solution containing acrylic acid, aminopropyl triethoxysilane, initiator I2959 and polyvinyl alcohol, and then dripping it on the BOPP corona film prepared in step (1), irradiating it under an LED ultraviolet curing lamp, soaking it in deionized water, rinsing it with ethanol, and then drying it to obtain a BOPP / PAA grafted film;

[0008] (3) Prepare a certain concentration of ethyl orthosilicate, concentrated hydrochloric acid, ammonium fluorotitanate, boric acid, water and ethanol silicate sol, and then apply it on the BOPP / PAA grafted film prepared in step (2). After room temperature reaction, ultrasonic cleaning with deionized water and ethanol is carried out in sequence, and the BOPP / SiO2@TiO2 nanocomposite film is obtained after drying.

[0009] Preferably, the power of the corona treater in step (1) is 1.0-3.0 W, preferably 1.5 W.

[0010] Preferably, in step (2), the mass ratio of acrylic acid, APTES, I2959 and PVA is 63:19:0.3:21:200.

[0011] Preferably, in step (2), the LED ultraviolet curing lamp has a wavelength of λ=365nm and a power of 20W.

[0012] Preferably, in step (3), the mass ratio of tetraethyl orthosilicate, concentrated hydrochloric acid, ammonium fluorotitanate, boric acid, water and ethanol is 20-95:12:1:0.9:70:53.

[0013] Preferably, the light transmittance of the nano-SiO2@TiO2 modified BOPP film prepared in step (3) is 80-90%.

[0014] Preferably, the thickness of the nano-SiO2@TiO2 modified BOPP film nano-coating prepared in step (3) is 2-6 μm.

[0015] Another object of the present invention is to provide an application of a nano-SiO2@TiO2 coating modified BOPP film, which can be used to print water-based ink on the nano-SiO2@TiO2 modified BOPP film with high precision and strong adhesion through a screen printing process.

[0016] Compared with the prior art, the advantages of the present invention are:

[0017] 1. Nano-SiO2@TiO2 coating can be easily prepared on BOPP film by adjusting the ratio of silicon to titanium. The preparation of BOPP / PAA grafted film by UV graft polymerization can further improve the adhesion of nano-SiO2@TiO2 coating to BOPP film, and obtain a firmly bonded BOPP / SiO2@TiO2 nanocomposite film.

[0018] 2. Based on the above unique structure, the BOPP / SiO2@TiO2 nanocomposite film significantly improves the wettability and bonding force of water-based ink on its surface. Compared with the water-based ink screen printing effect of other BOPP films, the nanocomposite film has been significantly improved in both printing accuracy and adhesion. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Optical photographs of the BOPP film, BOPP corona film, BOPP / PAA grafted film, and BOPP / SiO2@TiO2 nanocomposite film prepared in Example 1 of the present invention;

[0020] Figure 2 This is a SEM image of the surface of the BOPP corona film prepared in Example 2 of the present invention;

[0021] Figure 3 This is a SEM image of the surface of the BOPP / PAA grafted film prepared in Example 3 of the present invention;

[0022] Figure 4 This is a SEM image of the surface of the BOPP / SiO2@TiO2 nanocomposite film prepared in Example 3 of the present invention;

[0023] Figure 5 These are optical microscope photographs of the water-based ink printing surfaces of different types of BOPP films, BOPP corona films, BOPP / PAA grafted films, and BOPP / SiO2@TiO2 nanocomposite films prepared by screen printing technology in Example 3 of the present invention.

[0024] Figure 6 This is a SEM cross-sectional view of the three-layer composite structure of the BOPP / SiO2@TiO2 nanocomposite film prepared in Example 3 of the present invention obtained by screen printing process. DETAILED DESCRIPTION

[0025] The present invention is further described below through specific implementation modes, but the implementation modes of the present invention are not limited thereto.

[0026] Example 1

[0027] (1) The BOPP film is ultrasonically cleaned with deionized water and ethanol in sequence, and then dried and corona treated to obtain a BOPP corona film. Figure 1 This is the SEM image of the prepared BOPP corona film. It can be seen from the image that the surface is relatively smooth;

[0028] (2) Ultrasonic mixing of acrylic acid, APTES, I2959, PVA and water in a mass ratio of 63:19:0.3:21:200 was performed, and then an appropriate amount of prepolymer solution was dripped onto the BOPP corona film and irradiated under an LED UV curing lamp for 10 minutes to perform graft polymerization. After the reaction, the BOPP film was soaked in deionized water for 120 minutes, and finally rinsed with deionized water and ethanol three times, and dried to obtain a BOPP / PAA grafted film;

[0029] (3) Ethyl orthosilicate, concentrated hydrochloric acid, ammonium fluorotitanate, boric acid, water, and ethanol were mixed and dissolved in a mass ratio of 93:12:1:0.9:70:53, and the silicon-titanium sol was obtained by ultrasonication. The silicon-titanium mixed sol was scraped onto the BOPP / PAA grafted film, left to dry at 20°C for 2 hours, ultrasonically cleaned with deionized water and ethanol for 15 minutes, and finally dried to obtain the BOPP / SiO2@TiO2 nanocomposite film. Among them, Figure 1 (ad) are optical photographs of the prepared BOPP film, BOPP corona film, BOPP / PAA grafted film, and BOPP / SiO2@TiO2 nanocomposite film, respectively. All four films have high transparency, especially the transparency of the nano-coating modified composite film is maintained;

[0030] (4) The prepared BOPP / SiO2@TiO2 nanocomposite film was printed with water-based ink using a screen printing process, and then quickly dried at 50° in a vacuum oven for 2 h.

[0031] Example 2

[0032] (1) The BOPP film is ultrasonically cleaned with deionized water and ethanol in sequence, and then dried and corona treated to obtain a BOPP corona film. Figure 2 This is the SEM image of the surface of the prepared BOPP corona film. It can be seen from the image that the surface is relatively smooth;

[0033] (2) Ultrasonic mixing of acrylic acid, APTES, I2959, PVA and water in a mass ratio of 63:19:0.3:21:200 was performed, and then an appropriate amount of prepolymer droplets were applied to the BOPP corona film, and irradiated under an LED UV curing lamp for 10 minutes to carry out graft polymerization reaction. The BOPP film was soaked in deionized water for 120 minutes, and finally rinsed with deionized water and ethanol three times, and dried to obtain a BOPP / PAA grafted film;

[0034] (3) Ethyl orthosilicate, concentrated hydrochloric acid, ammonium fluorotitanate, boric acid, water, and ethanol were mixed and dissolved in a mass ratio of 23.5:12:1:0.9:70:53, and the silicon-titanium sol was obtained by ultrasonication. The silicon-titanium mixed sol was coated on the BOPP / PAA grafted film, left to dry at 20°C for 2 hours, ultrasonically cleaned with deionized water and ethanol for 15 minutes, and finally dried to obtain the BOPP / SiO2@TiO2 nanocomposite film;

[0035] (4) The prepared BOPP / SiO2@TiO2 nanocomposite film was printed with water-based ink using a screen printing process, and was quickly dried at 50° in a vacuum oven for 2 h to solidify.

[0036] Example 3

[0037] (1) The BOPP film is ultrasonically cleaned with deionized water and ethanol in sequence, and then dried and corona treated to obtain a BOPP corona film;

[0038] (2) Ultrasonic mixing of acrylic acid, APTES, I2959, PVA and water in a mass ratio of 63:19:0.3:21:200 was performed, and then an appropriate amount of prepolymer droplets were applied to the BOPP corona film, and irradiated under an LED UV curing lamp for 10 minutes to carry out graft polymerization reaction. The BOPP film was soaked in deionized water for 120 minutes, and finally rinsed with deionized water and ethanol three times, and dried to obtain a BOPP / PAA grafted film. Among them, Figure 3 This is the SEM image of the prepared BOPP grafted film. It can be seen from the image that there are obvious wrinkles on the surface;

[0039] (3) Ethyl orthosilicate, concentrated hydrochloric acid, ammonium fluorotitanate, boric acid, water, and ethanol were mixed and dissolved in a mass ratio of 47:12:1:0.9:70:53, and a silicon-titanium sol was obtained by ultrasonication. The prepared silicon-titanium mixed sol was scraped onto the BOPP / PAA grafted film, left to dry at 20°C for 2 hours, ultrasonically cleaned with deionized water and ethanol for 15 minutes, and finally dried to obtain a BOPP / SiO2@TiO2 nanocomposite film. Among them, Figure 4 The SEM image of the prepared BOPP / SiO2@TiO2 nanocomposite film shows that there are a large number of nanoparticles on the surface, which will be beneficial for the subsequent screen printing of water-based inks.

[0040] (4) Screen printing the BOPP / SiO2@TiO2 nanocomposite film with water-based ink, and then quickly drying it at 50° in vacuum for 2 hours to solidify it. Figure 5Optical micrographs of the water-based ink printed surfaces of different types of BOPP films, BOPP corona films, BOPP / PAA grafted films, and BOPP / SiO2@TiO2 nanocomposite films prepared by screen printing technology. Compared with other BOPP films, the nano-modified composite film has the best screen printing effect, with clear stripes and uniform ink distribution without obvious bubbles. Figure 6 This is the SEM cross-sectional image of the prepared BOPP / SiO2@TiO2 nanocomposite film printed with water-based ink. From the figure, it can be seen that the BOPP middle layer is a SiO2@TiO2 nanolayer with a thickness of about 2.5μm, and the upper water-based ink layer has a thickness of about 3.5μm. They are closely combined together and have a good printing effect.

[0041] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a nano-SiO2@TiO2 coating modified BOPP film, which has the following characteristics and comprises the following steps: (1) The BOPP film is ultrasonically cleaned with deionized water and ethanol in sequence, dried, and then corona pretreated to obtain a BOPP corona film; (2) preparing a prepolymer solution containing acrylic acid, aminopropyltriethoxysilane (APTES), initiator I2959 and polyvinyl alcohol, and then dripping it on the BOPP corona film prepared in step (1), and then irradiating it under an LED ultraviolet curing lamp for graft polymerization. After the reaction is completed, soaking it in deionized water, rinsing it with ethanol, and then drying it to obtain a BOPP film with polyacrylic acid (PAA) grafted on the surface, which is recorded as a BOPP / PAA grafted film; (3) preparing a certain concentration of silicon-titanium sol of tetraethyl orthosilicate, concentrated hydrochloric acid, ammonium fluorotitanate, boric acid, water and ethanol, and then coating it on the BOPP / PAA grafted film prepared in step (2), reacting at room temperature, ultrasonically cleaning with deionized water, and drying to obtain a BOPP composite film modified with a nano-SiO2@TiO2 coating, i.e., a BOPP / SiO2@TiO2 nano-composite film.

2. The method for preparing a nano-SiO2@TiO2 coating modified BOPP film according to claim 1, characterized in that: The corona power of step (1) is 1.0-3.0W.

3. The method for preparing a nano-SiO2@TiO2 coating modified BOPP film according to claim 1, characterized in that: The mass ratio of acrylic acid, APTES, I2959, PVA and water in step (2) is 63:19:0.3:21:

200.

4. The method for preparing a nano-SiO2@TiO2 coating modified BOPP film according to claim 1, characterized in that: The LED ultraviolet curing lamp in step (2) has a wavelength of λ=365nm and a power of 20W.

5. The method for preparing a nano-SiO2@TiO2 coating modified BOPP film according to claim 1, characterized in that: The mass ratio of the tetraethyl orthosilicate, concentrated hydrochloric acid, ammonium fluorotitanate, boric acid, water and ethanol in step (3) is 20-95:12:1:0.9:70:

53.

6. The method for preparing a nano-SiO2@TiO2 coating modified BOPP film according to claim 1, characterized in that: The light transmittance of the nano-SiO2@TiO2 modified BOPP film described in step (3) is 80-90%.

7. The method for preparing a nano-SiO2@TiO2 coating modified BOPP film according to claim 1, characterized in that: The thickness of the nano-SiO2@TiO2 modified BOPP film nano-coating described in step (3) is 2-6 μm.

8. A nano-SiO2@TiO2 coating modified BOPP film, characterized in that: Obtained by the preparation method described in claims 1-7.

9. The use of a nano-SiO2@TiO2 coating modified BOPP composite film according to claim 8 or 1-7, characterized in that: Through the screen printing process, the water-based ink is printed on the nano-SiO2@TiO2 modified BOPP composite film with high precision and strong adhesion.

Citation Information

Cited By

  • High-shrinkage BOPP printing film and preparation method thereof

    CN121554804A