Preparation method of multifunctional polyethylene pipe for plastic-lined composite pipe

By adding boron nitride reinforcement and composite antibacterial additives to polyethylene pipes, the problem of insufficient mechanical properties and antibacterial properties of plastic-lined composite pipes in the water supply system is solved, and the improvement of high mechanical properties and antibacterial properties is achieved, which extends the Service life.

CN118931011AActive Publication Date: 2024-11-12GUANGDONG LUCKY PYLON CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411177611.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Plastic-lined composite pipes need to improve mechanical properties and antibacterial properties in water supply systems to avoid damage and bacterial corrosion and extend service life.

Method used

Using the high-density polyethylene pipe preparation method, boron nitride reinforcement and composite antibacterial additives are added, and boron nitride reinforcement and composite antibacterial additives are prepared through hydrothermal reaction and ultrasound to improve the compatibility of polyvinyl matrix and Antibacterial properties and cross-linking network structures are formed through cross-linking agents to enhance mechanical properties and toughness.

Benefits of technology

The prepared polyethylene pipe has high tensile strength, bending elastic modulus and impact strength, and has an antibacterial rate of up to 99.99%, meeting the application needs of water supply systems and having a long service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931011A_ABST
    Figure CN118931011A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer materials, and discloses a preparation method of a multifunctional polyethylene pipe for a plastic-lined composite pipe, the polyethylene pipe comprises the following raw materials: high-density polyethylene, a boron nitride reinforcing material, a composite antibacterial additive, a cross-linking agent, an antioxidant and a lubricant; high-density polyethylene is used as a matrix material, and a boron nitride reinforcing material is added, so that the interaction force and binding force with a polyethylene matrix are enhanced, external impact energy is absorbed and dispersed, crack propagation is hindered, and the mechanical property and toughness of the polyethylene pipe are improved; by adding the composite antibacterial additive, the antibacterial performance of the polyethylene pipe is improved, the polyethylene pipe can show excellent antibacterial performance only by adding a small amount of the composite antibacterial additive, bacteria can be effectively prevented from being attached to the surface of a pipeline material to generate a corrosion effect, and the service life of the polyethylene pipe is further prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a method for preparing a multifunctional polyethylene pipe for a plastic-lined composite pipe. Background Art

[0002] With the rapid development of industrialization, the demand for pipeline materials is also increasing. As a new type of pipe, the plastic-lined composite pipe combines the advantages of metal and plastic. The composite structure of the plastic-lined composite pipe makes up for the shortcomings of a single material, improves the overall performance of the pipe, and has multiple uses. It has gradually become one of the most popular pipes in the market. It is widely used in water supply systems, chemical industry, environmental protection treatment systems, oil and gas transportation, agricultural irrigation, heating systems, fire protection systems, marine engineering and other fields. Common plastic-lined composite pipes include aluminum alloy plastic-lined composite pipes, steel plastic-lined composite pipes, etc. Metal pipes are used as the main supporting structure of the pipeline, and plastic pipes are on the inner wall or outer wall or both; plastic pipes are usually made of polyvinyl chloride, polypropylene, polyethylene and other materials. Among them, polyethylene has excellent corrosion resistance and can ensure long-term stable operation. When used in water supply systems, it is odorless and non-toxic, and will not affect the water quality, which can ensure the safety and sanitation of water quality. In addition, polyethylene has a smooth surface and a small friction coefficient, and it will not easily accumulate scale. On the one hand, it ensures the sanitation, and on the other hand, it improves the transportation efficiency and reduces energy consumption. Therefore, polyethylene is often used to make plastic pipes for plastic-lined composite pipes.

[0003] When plastic-lined composite pipes are used in water supply systems, plastic pipes need to withstand internal and external pressures, and stress concentration may cause damage to the pipes. In order to ensure the long-term safe operation of the pipes, the mechanical properties and toughness need to be enhanced to effectively avoid pipe deformation and cracking. At the same time, as the part that is in direct contact with domestic water, bacteria can easily adhere to the inner wall of the pipes, which can corrode the pipe materials and pollute domestic water. In order to reduce the damage of bacteria to the pipes, plastic pipes need to have antibacterial properties, which can extend the service life of plastic pipes to a certain extent, ensure the safety of water quality, and improve the reliability and stability of the water supply system. Summary of the invention

[0004] In order to solve the problems mentioned in the background technology, the purpose of the present invention is to provide a method for preparing a multifunctional polyethylene pipe for a plastic-lined composite pipe.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A method for preparing a multifunctional polyethylene pipe for a plastic-lined composite pipe comprises the following steps:

[0007] Step 1: Add 80-100 parts of high-density polyethylene, 4-6 parts of boron nitride reinforcement, 3-5 parts of composite antibacterial additives, 1-3 parts of cross-linking agent, 0.5-1.5 parts of antioxidant, and 1-3 parts of lubricant into a high-speed mixer according to weight parts, set the speed to 500-800r / min, increase the temperature to 100-140°C, mix and stir for 10-30min, and when the material temperature is cooled to 30-40°C, discharge the material to obtain a mixed base material;

[0008] Step 2: Add the mixed base material to a twin-screw extruder, set the screw speed of the twin-screw extruder to 30-60r / min, extrude through the twin-screw extruder, cool and shape, and obtain a polyethylene pipe.

[0009] Furthermore, in step one, the cross-linking agent is diisopropyl peroxide or di-tert-butyl peroxide; the antioxidant is antioxidant 1076 and antioxidant 168 in a mass ratio of 1:1; and the lubricant is any one of polyethylene wax, paraffin or zinc stearate.

[0010] Furthermore, in step 2, the temperature of zone 1 of the twin-screw extruder is 160-180°C, the temperature of zone 2 is 170-190°C, the temperature of zone 3 is 180-200°C, the temperature of zone 4 is 200-220°C, and the temperature of zone 5 is 220-230°C.

[0011] Furthermore, the preparation method of the boron nitride reinforcement material comprises the following steps:

[0012] Step A, adding hexagonal boron nitride to an ethanol solution with a volume fraction of 55%-60%, ultrasonically treating for 10-30 minutes, adding the solution to a hydrothermal reactor, reacting at a temperature of 140-160° C. for 5-8 hours, cooling, centrifuging, precipitating, and vacuum drying to obtain hydroxylated hexagonal boron nitride;

[0013] Step B, adding hydroxylated hexagonal boron nitride to dimethyl sulfoxide, ultrasonicating for 10-30 minutes to form a uniform dispersion, introducing nitrogen, adding terminal isocyanate polybutadiene and a catalyst to the dispersion, raising the temperature to 85-95° C., keeping the reaction warm for 4-6 hours, filtering, washing the solid product, and vacuum drying to obtain a boron nitride reinforcement material.

[0014] Furthermore, in step A, the average particle size of the hexagonal boron nitride is 120 nm.

[0015] Furthermore, in step B, the catalyst is dibutyltin dilaurate or stannous octoate.

[0016] By adopting the above technical scheme, during the hydrothermal reaction of hexagonal boron nitride, boiling water accelerates the hydrolysis of hexagonal boron nitride to obtain hydroxylated hexagonal boron nitride. Under the action of the catalyst, the active hydroxyl groups in the hydroxylated hexagonal boron nitride react with the isocyanate groups in the terminal isocyanate polybutadiene structure to obtain a boron nitride reinforcement. The boron nitride reinforcement material is prepared by organically modifying hexagonal boron nitride and grafting hexagonal boron nitride with polybutadiene, so as to build a molecular bridge between the interface of hexagonal boron nitride and polyethylene, improve the compatibility between the two, and thus avoid the agglomeration problem of hexagonal boron nitride in the polyethylene matrix, so that the hexagonal boron nitride is evenly dispersed and orderly arranged in the polyethylene matrix, and the interaction force and bonding force between the hexagonal boron nitride and the polyethylene molecular chain are enhanced, so that the polyethylene pipe can bear the load more evenly when subjected to external force, effectively disperse and transfer stress, and improve the mechanical properties. At the same time, the polybutadiene molecular chain can absorb and disperse external impact energy, hinder crack propagation, reduce the degree of damage to the polyethylene matrix caused by stress concentration, and enhance the toughness of the polyethylene matrix. In addition, under the action of the cross-linking agent, the polybutadiene molecular chain in the structure of the boron nitride reinforcement material can be cross-linked with the polyethylene matrix polymer chain segment to form a cross-linked network structure, further enhancing the mechanical properties and toughness of the polyethylene matrix, so that the polyethylene pipe exhibits higher mechanical properties.

[0017] Furthermore, the preparation method of the composite antibacterial additive is as follows:

[0018] Konjac glucomannan is added to N,N-dimethylformamide, stirred evenly, and then baicalin and a composite catalyst are added. The reaction is carried out at room temperature for 4-6 hours. The product is collected, washed, and dried at 40-50° C. to a constant weight to obtain a composite antibacterial additive.

[0019] By adopting the above technical scheme, a large number of active hydroxyl groups in the structure of konjac glucomannan can undergo esterification reaction with active carboxyl groups in the structure of baicalin under the action of a composite catalyst, thereby introducing the natural antibacterial substance baicalin into the structure of konjac glucomannan to obtain a composite antibacterial additive. The composite antibacterial additive contains baicalin, a flavonoid antibacterial substance. Baicalin, as a natural antibacterial substance, has a broad-spectrum antibacterial effect and can make the polyethylene matrix have excellent antibacterial properties. In addition, after konjac glucomannan is an environmentally friendly natural macromolecular organic matter and is grafted with baicalin, the precipitation of small molecule baicalin antibacterial substances can be effectively avoided, and the antibacterial properties are excellent. Only a small amount of composite antibacterial additives need to be added to the polyethylene matrix to make the polyethylene pipe have a lasting antibacterial effect, effectively avoiding the attachment of bacteria on the surface of the pipeline material and the corrosion of the pipeline material, thereby extending the service life of the polyethylene pipe.

[0020] Furthermore, the composite catalyst is 4-dimethylaminopyridine and dicyclohexylcarbodiimide in a mass ratio of 2-3:6-8.

[0021] Beneficial effects of the present invention:

[0022] The present invention prepares a boron nitride reinforcing material and a composite antibacterial additive and adds them to a polyethylene matrix material, so that the prepared polyethylene pipe has a tensile strength of up to 32.5MPa, a bending elastic modulus of up to 81.8MPa, and an impact strength of up to 26.5KJ / m 2 The antibacterial rate is as high as 99.99%. It has excellent mechanical properties, toughness and antibacterial properties. It can meet the application requirements of polyethylene as a lined plastic composite pipe in the water supply system and has a long service life.

[0023] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0025] Figure 1 is an infrared spectrum of the boron nitride reinforcement material in the embodiment of the present invention;

[0026] Figure 2 It is the infrared spectrum of konjac glucomannan and composite antibacterial additive in the embodiment of the present invention. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] 1. Preparation of Boron Nitride Reinforcement Material

[0030] Step A, adding 2 g of hexagonal boron nitride with an average particle size of 120 nm to an ethanol solution with a volume fraction of 55%, ultrasonically treating for 20 minutes, adding the solution to a hydrothermal reactor, reacting at 160° C. for 6 hours, cooling, centrifuging, precipitating, and vacuum drying to obtain hydroxylated hexagonal boron nitride;

[0031] Step B, add 2g of hydroxylated hexagonal boron nitride to dimethyl sulfoxide, ultrasonicate for 20min to form a uniform dispersion, introduce nitrogen, add 1.2g of terminal isocyanate polybutadiene and 0.2g of dibutyltin dilaurate to the dispersion, increase the temperature to 90°C, keep the reaction for 5h, filter, wash the solid product, and vacuum dry to obtain a boron nitride reinforcement.

[0032] The sample was prepared by potassium bromide tableting method, and the boron nitride reinforced material was tested by infrared spectrometer. Figure 1 As shown, the spectral wavenumber test range is 4000cm -1 -500cm -1 , analysis shows that in the infrared spectrum of boron nitride reinforcement, 3021cm -1 The absorption peak of CH in the double bond appears at 1715 cm -1 The absorption peak of C=O in carbamate appeared at 1536 cm -1 The absorption peak of NH appeared at 1378 cm -1 The absorption peak of BN appears at 807 cm -1 The absorption peak of BNB appears at

[0033] 2. Preparation of composite antibacterial additives

[0034] 2.5 g of konjac glucomannan was added to N,N-dimethylformamide, and after stirring evenly, 4.2 g of baicalin, 0.3 g of 4-dimethylaminopyridine and 0.8 g of dicyclohexylcarbodiimide were added, and the reaction was carried out at room temperature for 5 h. The product was collected, washed, and dried at 45°C to constant weight to obtain a composite antibacterial additive.

[0035] The potassium bromide tableting method was used to prepare the samples, and the konjac glucomannan and the composite antibacterial additives were tested by infrared spectroscopy. Figure 2 As shown, the spectral wavenumber test range is 4000cm -1 -500cm -1 According to the analysis, in the infrared spectrum of konjac glucomannan, 1727cm -1 The absorption peak of C=O in acetyl group appeared at 1065cm -1 The absorption peak of COC appeared at 890 cm -1 The absorption peak of β-1,4 glycosidic bond appeared at 1750cm -1 The area of ​​the C=O absorption peak at 1715 cm -1 The absorption peak of the carbonyl group C=O at position 4 of baicalin appeared at 1608 cm -1 、1571cm -1 、1494cm-1 The absorption peak is the skeleton of baicalin.

[0036] 3. Preparation of polyethylene pipes

[0037] Step 1, add 80g high-density polyethylene, 4g boron nitride reinforcement, 3g composite antibacterial additive, 1g diisopropyl peroxide, 0.25g antioxidant 1076, 0.25g antioxidant 168, and 1g polyethylene wax into a high-speed mixer, set the speed to 500r / min, increase the temperature to 100°C, mix and stir for 10min, and when the material temperature is cooled to 30°C, discharge the material to obtain a mixed base material;

[0038] Step 2: Add the mixed base material to a twin-screw extruder, set the screw speed of the twin-screw extruder to 30 r / min, the temperature of zone 1 of the twin-screw extruder to 160°C, the temperature of zone 2 to 170°C, the temperature of zone 3 to 180°C, the temperature of zone 4 to 200°C, and the temperature of zone 5 to 220°C. Extrude through the twin-screw extruder, cool and shape, and obtain a polyethylene pipe.

[0039] Example 2

[0040] Preparation of polyethylene pipes

[0041] Step 1, add 90g high-density polyethylene, 5g boron nitride reinforcement prepared in Example 1, 4g composite antibacterial additive prepared in Example 1, 2g diisopropyl peroxide, 0.5g antioxidant 1076, 0.5g antioxidant 168, and 2g polyethylene wax into a high-speed mixer, set the speed to 650r / min, increase the temperature to 125°C, mix and stir for 20min, and when the material temperature is cooled to 35°C, discharge the material to obtain a mixed base material;

[0042] Step 2: Add the mixed base material to a twin-screw extruder, set the screw speed of the twin-screw extruder to 45r / min, the temperature of zone 1 of the twin-screw extruder to 170°C, the temperature of zone 2 to 180°C, the temperature of zone 3 to 190°C, the temperature of zone 4 to 210°C, and the temperature of zone 5 to 225°C. After extrusion through the twin-screw extruder and cooling and shaping, a polyethylene pipe is obtained.

[0043] Example 3

[0044] Preparation of polyethylene pipes

[0045] Step 1, add 100g high-density polyethylene, 6g boron nitride reinforcement prepared in Example 1, 5g composite antibacterial additive prepared in Example 1, 3g diisopropyl peroxide, 0.75g antioxidant 1076, 0.75g antioxidant 168, and 3g polyethylene wax into a high-speed mixer, set the speed to 800r / min, increase the temperature to 140°C, mix and stir for 30min, and when the material temperature is cooled to 40°C, discharge the material to obtain a mixed base material;

[0046] Step 2: Add the mixed base material to a twin-screw extruder, set the screw speed of the twin-screw extruder to 60r / min, the temperature of zone 1 of the twin-screw extruder to 180°C, the temperature of zone 2 to 190°C, the temperature of zone 3 to 200°C, the temperature of zone 4 to 220°C, and the temperature of zone 5 to 230°C. Extrude through the twin-screw extruder, cool and shape, and obtain a polyethylene pipe.

[0047] Comparative Example 1

[0048] Preparation of polyethylene pipes

[0049] Step 1, add 90g high-density polyethylene, 5g boron nitride reinforcement prepared in Example 1, 2g diisopropyl peroxide, 0.5g antioxidant 1076, 0.5g antioxidant 168, and 2g polyethylene wax into a high-speed mixer, set the speed to 650r / min, increase the temperature to 125°C, mix and stir for 20min, and when the material temperature is cooled to 35°C, discharge the material to obtain a mixed base material;

[0050] Step 2: Add the mixed base material to a twin-screw extruder, set the screw speed of the twin-screw extruder to 45r / min, the temperature of zone 1 of the twin-screw extruder to 170°C, the temperature of zone 2 to 180°C, the temperature of zone 3 to 190°C, the temperature of zone 4 to 210°C, and the temperature of zone 5 to 225°C. After extrusion through the twin-screw extruder and cooling and shaping, a polyethylene pipe is obtained.

[0051] Comparative Example 2

[0052] Preparation of polyethylene pipes

[0053] Step 1, add 90g high-density polyethylene, 4g of the composite antibacterial additive prepared in Example 1, 2g of diisopropyl peroxide, 0.5g of antioxidant 1076, 0.5g of antioxidant 168, and 2g of polyethylene wax into a high-speed mixer, set the speed to 650r / min, increase the temperature to 125°C, mix and stir for 20min, and when the material temperature is cooled to 35°C, discharge the material to obtain a mixed base material;

[0054] Step 2: Add the mixed base material to a twin-screw extruder, set the screw speed of the twin-screw extruder to 45r / min, the temperature of zone 1 of the twin-screw extruder to 170°C, the temperature of zone 2 to 180°C, the temperature of zone 3 to 190°C, the temperature of zone 4 to 210°C, and the temperature of zone 5 to 225°C. After extrusion through the twin-screw extruder and cooling and shaping, a polyethylene pipe is obtained.

[0055] Comparative Example 3

[0056] Preparation of polyethylene pipes

[0057] Step 1, add 90g high-density polyethylene, 5g hexagonal boron nitride, 4g of the composite antibacterial additive prepared in Example 1, 2g diisophenyl peroxide, 0.5g antioxidant 1076, 0.5g antioxidant 168, and 2g polyethylene wax into a high-speed mixer, set the speed to 650r / min, increase the temperature to 125°C, mix and stir for 20min, and when the material temperature is cooled to 35°C, discharge the material to obtain a mixed base material;

[0058] Step 2: Add the mixed base material to a twin-screw extruder, set the screw speed of the twin-screw extruder to 45r / min, the temperature of zone 1 of the twin-screw extruder to 170°C, the temperature of zone 2 to 180°C, the temperature of zone 3 to 190°C, the temperature of zone 4 to 210°C, and the temperature of zone 5 to 225°C. After extrusion through the twin-screw extruder and cooling and shaping, a polyethylene pipe is obtained.

[0059] Comparative Example 4

[0060] Preparation of polyethylene pipes

[0061] Step 1, add 90g high-density polyethylene, 5g boron nitride reinforcement prepared in Example 1, 4g baicalin, 2g diisophenyl peroxide, 0.5g antioxidant 1076, 0.5g antioxidant 168, and 2g polyethylene wax into a high-speed mixer, set the speed to 650r / min, increase the temperature to 125°C, mix and stir for 20min, and when the material temperature is cooled to 35°C, discharge the material to obtain a mixed base material;

[0062] Step 2: Add the mixed base material to a twin-screw extruder, set the screw speed of the twin-screw extruder to 45r / min, set the temperature of zone 1 to 170°C, the temperature of zone 2 to 180°C, the temperature of zone 3 to 190°C, the temperature of zone 4 to 210°C, and the temperature of zone 5 to 225°C. Extrude through the twin-screw extruder, cool and shape, and obtain a polyethylene pipe.

[0063] Performance Testing

[0064] The polyethylene pipes prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were made into specimens that met the test specifications and were tested for performance:

[0065] According to the standard GB / T 1040.1-2018, the tensile properties of the test strips were tested; according to the standard GB / T 9341-2008, the bending elastic modulus of the test strips was tested; according to the standard GB / T1843-2008, the impact strength of the test strips was tested; according to the standard GB / T31402-2023, the antibacterial properties of the test strips were tested after the test strips were placed at room temperature for 20 days. The results are shown in the following table:

[0066]

[0067] As can be seen from the above table, the polyethylene pipes prepared by Examples 1 to 3 of the present invention have excellent mechanical properties, toughness and antibacterial properties. Comparative Example 1 did not add the composite antibacterial additive, and the antibacterial property test results were poor; Comparative Example 2 did not add the boron nitride reinforcement, and the tensile strength, bending elastic modulus and impact strength test results were poor; Comparative Example 3 added unmodified hexagonal boron nitride, which has the effect of enhancing mechanical properties, but it is easy to agglomerate in the polyethylene matrix, resulting in poor tensile strength test results, and it is impossible to use polybutadiene to graft hexagonal boron nitride to enhance the toughness of polyethylene pipes, and cross-link with the polyethylene matrix to further enhance mechanical properties and toughness, so the tensile strength, bending elastic modulus and impact strength test results are poor; Comparative Example 4 added baicalin, but was not grafted with high molecular weight konjac glucomannan, and small molecule baicalin may precipitate in the polyethylene matrix, resulting in reduced antibacterial properties, so the antibacterial rate test result is poor.

[0068] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a multifunctional polyethylene pipe for a plastic-lined composite pipe, characterized in that: The following steps are involved: Step 1: Add 80-100 parts of high-density polyethylene, 4-6 parts of boron nitride reinforcement, 3-5 parts of composite antibacterial additives, 1-3 parts of cross-linking agent, 0.5-1.5 parts of antioxidant, and 1-3 parts of lubricant into a high-speed mixer according to weight parts, set the speed to 500-800r / min, increase the temperature to 100-140°C, mix and stir for 10-30min, and when the material temperature is cooled to 30-40°C, discharge the material to obtain a mixed base material; Step 2: Add the mixed base material to a twin-screw extruder, set the screw speed of the twin-screw extruder to 30-60r / min, extrude through the twin-screw extruder, cool and shape, and obtain a polyethylene pipe.

2. The method for preparing a multifunctional polyethylene pipe for a plastic-lined composite pipe according to claim 1, characterized in that: In step 1, the cross-linking agent is diisopropyl peroxide or di-tert-butyl peroxide; the antioxidant is antioxidant 1076 and antioxidant 168 in a mass ratio of 1:1; and the lubricant is any one of polyethylene wax, paraffin or zinc stearate.

3. The method for preparing a multifunctional polyethylene pipe for a plastic-lined composite pipe according to claim 1, characterized in that: In step 2, the temperature of zone 1 of the twin-screw extruder is 160-180°C, the temperature of zone 2 is 170-190°C, the temperature of zone 3 is 180-200°C, the temperature of zone 4 is 200-220°C, and the temperature of zone 5 is 220-230°C.

4. The method for preparing a multifunctional polyethylene pipe for a plastic-lined composite pipe according to claim 1, characterized in that: The preparation method of the boron nitride reinforcing material comprises the following steps: Step A, adding hexagonal boron nitride to an ethanol solution with a volume fraction of 55%-60%, ultrasonically treating for 10-30 minutes, adding the solution to a hydrothermal reactor, reacting at a temperature of 140-160° C. for 5-8 hours, cooling, centrifuging, precipitating, and vacuum drying to obtain hydroxylated hexagonal boron nitride; Step B, adding hydroxylated hexagonal boron nitride to dimethyl sulfoxide, ultrasonicating for 10-30 minutes to form a uniform dispersion, introducing nitrogen, adding terminal isocyanate polybutadiene and a catalyst to the dispersion, raising the temperature to 85-95° C., keeping the reaction warm for 4-6 hours, filtering, washing the solid product, and vacuum drying to obtain a boron nitride reinforcement material.

5. The method for preparing a multifunctional polyethylene pipe for a plastic-lined composite pipe according to claim 4, characterized in that: In step A, the average particle size of the hexagonal boron nitride is 120 nm.

6. The method for preparing a multifunctional polyethylene pipe for a plastic-lined composite pipe according to claim 4, characterized in that: In step B, the catalyst is dibutyltin dilaurate or stannous octoate.

7. The method for preparing a multifunctional polyethylene pipe for a plastic-lined composite pipe according to claim 1, characterized in that: The preparation method of the composite antibacterial additive is as follows: Konjac glucomannan is added to N,N-dimethylformamide, stirred evenly, and then baicalin and a composite catalyst are added. The reaction is carried out at room temperature for 4-6 hours. The product is collected, washed, and dried at 40-50° C. to a constant weight to obtain a composite antibacterial additive.

8. The method for preparing a multifunctional polyethylene pipe for a plastic-lined composite pipe according to claim 7, characterized in that: The composite catalyst is 4-dimethylaminopyridine and dicyclohexylcarbodiimide in a mass ratio of 2-3:6-8.

Citation Information

Patent Citations

  • Antibacterial, ratproof and ultraviolet-proof PE gas pipeline

    CN106566052A

  • Safe, bacterium-inhibition and environment-friendly fruit and vegetable fresh-keeping film and preparation method thereof

    CN108384092A

  • Antibacterial plastic bottle as well as preparation method and application thereof

    CN109503928A

  • Anti-static and flame-retarding PE pipe and preparing method thereof

    CN110172196A

  • High-thermal-conductivity boron nitride modified insulating rubber composite material and preparation method thereof

    CN111333925A