Composite material based on styrene-maleic anhydride copolymer and application thereof
By pretreating hydrated metal oxide flame retardant and grafting agent to treat aluminosilicates, a spatial network structure is formed, which improves the flame retardant and electrical properties of composite materials based on styrene-maleic anhydride copolymer, and solves the problem of current The problem of insufficient flame retardancy of materials has achieved the comprehensive performance improvement of the three-electric system of new energy vehicles.
Patent Information
- Application Number
- CN202411178635.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
The existing three-electric system materials based on styrene-maleic anhydride copolymer are insufficient in new energy vehicles and are difficult to meet the strict performance requirements.
The aluminosilicate is treated with pretreated hydrated metal oxide flame retardant and grafting agent to form a stable spatial network structure, improve the flame retardant and electrical properties of the material, and improve the mechanical properties through coupling agents.
It realizes excellent flame retardant performance, smoke suppression effect and good mechanical properties of composite materials, and meets the comprehensive performance requirements of the three-electric system of new energy vehicles.
Smart Images

Figure CN118931081A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer materials, and in particular to a composite material based on styrene-maleic anhydride copolymer and its application. Background Art
[0002] New energy vehicles have been rapidly developed and popularized, especially the three-electric system has become the embodiment of the core technology of new energy vehicles. When selecting materials for the three-electric system, different car companies have different technical strategies. European and American car companies often use polyamides as the first choice for three-electric materials, Japanese car companies often use polyphenylene sulfide as the first choice for three-electric materials, and domestic car companies have both. The three-electric system materials have strict performance requirements. They must have high flame retardant and dielectric properties, as well as good dielectric tolerance, environmental temperature resistance and dimensional stability. SMA (styrene-maleic anhydride copolymer) is a non-crystalline polymer with good corrosion resistance and chemical stability, as well as good electrical insulation properties. It can be used for new energy vehicle three-electric system materials. However, due to the flammable styrene component contained in SMA, its flame retardancy cannot meet the requirements of the three-electric system of new energy vehicles. When used in the three-electric system of new energy vehicles, its flame retardancy needs to be improved.
[0003] At present, the focus is on improving and optimizing the mechanical properties, anti-noise and dimensional stability of SMA materials. At present, there is no flame-retardant SMA composite material technology for the three-electric system of new energy vehicles. It is urgent to develop an SMA composite material that meets the flame retardancy and electrical performance requirements of the three-electric system of new energy vehicles and has good mechanical properties. Summary of the invention
[0004] The present application provides a composite material based on styrene-maleic anhydride copolymer and its application to solve the following technical problem: how to improve the comprehensive performance of the composite material based on styrene-maleic anhydride copolymer.
[0005] In a first aspect, the present application provides a composite material based on styrene-maleic anhydride copolymer, wherein the raw material components of the composite material include:
[0006] a first base resin and a pretreated hydrated metal oxide flame retardant;
[0007] The first base resin includes styrene-maleic anhydride copolymer, and the pretreated hydrated metal oxide flame retardant is obtained by pretreating the hydrated metal oxide flame retardant with a coupling agent.
[0008] Optionally, the hydrated metal oxide flame retardant includes at least one of the following: aluminum hydroxide, magnesium hydroxide; and / or the coupling agent includes at least one of the following: borate, phosphate, titanate, aluminate, silane, stannate, zirconate.
[0009] Optionally, the pretreated hydrated metal oxide flame retardant is obtained by pretreating the hydrated metal oxide flame retardant with a coupling agent, comprising:
[0010] The preparation method of the pretreated hydrated metal oxide flame retardant is as follows:
[0011] Under the condition of set temperature, the hydrated metal oxide flame retardant is stirred, and a coupling agent is added to the hydrated metal oxide flame retardant in stages to obtain a pretreated hydrated metal oxide flame retardant; wherein,
[0012] In the pretreated hydrated metal oxide flame retardant, the hydrated metal oxide flame retardant is 5 to 15 parts by weight, and the coupling agent is 1.5 to 3 parts by weight.
[0013] Optionally, the set temperature is 115°C to 120°C.
[0014] Optionally, the raw material components of the composite material further include: a filler, and the filler is obtained by surface treating aluminosilicate with a grafting agent.
[0015] Optionally, the grafting agent includes at least one of the following: maleic anhydride grafted polypropylene wax, aminosilane, aminoacetate; and / or,
[0016] The aluminosilicate includes at least one of the following: quartz powder, phlogopite powder, and muscovite powder.
[0017] Optionally, the filler is obtained by surface treating aluminosilicate with a grafting agent, including:
[0018] The preparation method of the filler is as follows:
[0019] drying the aluminosilicate;
[0020] The dried aluminosilicate is mixed with a grafting agent to obtain a filler; wherein, in the filler, the aluminosilicate accounts for 10 to 20 parts by weight, and the grafting agent accounts for 5% to 6% of the weight of the aluminosilicate.
[0021] Optionally, the drying temperature is 115° C. to 120° C.; and / or,
[0022] The mixing temperature is 170°C to 175°C.
[0023] Optionally, the raw material components of the composite material also include: a second matrix resin and an auxiliary agent.
[0024] In a second aspect, the present application provides an application of a composite material based on styrene-maleic anhydride copolymer as described in any embodiment of the first aspect in a new energy vehicle.
[0025] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0026] The composite material based on styrene-maleic anhydride copolymer provided in an embodiment of the present application comprises raw material components including: a first base resin and a pretreated hydrated metal oxide flame retardant; the first base resin comprises a styrene-maleic anhydride copolymer, and the pretreated hydrated metal oxide flame retardant is obtained by pretreating the hydrated metal oxide flame retardant with a coupling agent. The hydrated metal oxide flame retardant has the advantages of no secondary pollution and good thermal stability. After the hydrated metal oxide flame retardant is pretreated with a coupling agent, the hydrated metal oxide flame retardant in the pretreated hydrated metal oxide flame retardant and the coupling agent can have a good interface connection effect, thereby improving the compatibility of the hydrated metal oxide flame retardant with the matrix resin styrene-maleic anhydride copolymer and the dispersibility of the hydrated metal oxide flame retardant in the matrix resin styrene-maleic anhydride copolymer, so that the pretreated hydrated metal oxide flame retardant is stably and evenly dispersed in the matrix resin styrene-maleic anhydride copolymer; the coupling agent makes up for the shortcomings of the mechanical properties of the hydrated metal oxide flame retardant and avoids a single flame retardant from destroying other properties of the composite material; the pretreated hydrated metal oxide flame retardant can not only improve the impact resistance of the composite material, but also achieve a good flame retardant effect, which means that the composite material maximizes the effect of the flame retardant to a certain extent while taking into account other properties of the composite material. Therefore, when the composite material is heated and burned and decomposed, the hydrated metal oxide flame retardant fully decomposes and undergoes a dehydration reaction, absorbing the heat on the surface of the styrene-maleic anhydride copolymer resin, thereby reducing the surface temperature of the styrene-maleic anhydride copolymer, and at the same time, dehydration produces a large amount of water vapor, which can dilute the concentration of combustible gas, and decomposes to produce dense residual metal oxides, which are deposited on the surface of the styrene-maleic anhydride copolymer plastic, limiting the generation of combustible gas, playing a role of heat insulation and oxygen isolation, and achieving the effect of smoke suppression, while the hydrated metal oxide can also improve the dielectric properties of the matrix resin. Therefore, the coupling agent cooperates with the hydrated metal oxide flame retardant to make the composite material of styrene-maleic anhydride copolymer have excellent flame retardant properties, while taking into account other properties of the composite material, which is ultimately reflected in improving the comprehensive performance of the composite material based on styrene-maleic anhydride copolymer. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0028] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0029] Figure 1 A schematic flow chart of a method for preparing a composite material based on styrene-maleic anhydride copolymer provided in an embodiment of the present application. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0031] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0032] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.
[0033] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0034] In a first aspect, the present application provides a composite material based on styrene-maleic anhydride copolymer, wherein the raw material components of the composite material include:
[0035] a first base resin and a pretreated hydrated metal oxide flame retardant;
[0036] The first base resin includes styrene-maleic anhydride copolymer (SMA), and the pretreated hydrated metal oxide flame retardant is obtained by pretreating the hydrated metal oxide flame retardant with a coupling agent.
[0037] In the embodiments of the present application, the hydrated metal oxide flame retardant has the advantages of no secondary pollution and good thermal stability. After the hydrated metal oxide flame retardant is pretreated with a coupling agent, the hydrated metal oxide flame retardant in the pretreated hydrated metal oxide flame retardant and the coupling agent can have a good interface connection effect, thereby improving the compatibility of the hydrated metal oxide flame retardant with the matrix resin styrene-maleic anhydride copolymer and the dispersibility of the hydrated metal oxide flame retardant in the matrix resin styrene-maleic anhydride copolymer, so that the pretreated hydrated metal oxide flame retardant is stably and evenly dispersed in the matrix resin styrene-maleic anhydride copolymer; the coupling agent makes up for the shortcomings of the mechanical properties of the hydrated metal oxide flame retardant and avoids a single flame retardant from destroying other properties of the composite material; the pretreated hydrated metal oxide flame retardant can not only improve the impact resistance of the composite material, but also achieve a good flame retardant effect, which means that the composite material maximizes the effect of the flame retardant to a certain extent while taking into account other properties of the composite material. Therefore, when the composite material is heated and burned and decomposed, the hydrated metal oxide flame retardant is fully decomposed to undergo a dehydration reaction, absorbing heat from the surface of the styrene-maleic anhydride copolymer resin, thereby reducing the surface temperature of the styrene-maleic anhydride copolymer. At the same time, dehydration produces a large amount of water vapor, which can dilute the concentration of combustible gas. In addition, decomposition produces dense residual metal oxides, which are deposited on the surface of the styrene-maleic anhydride copolymer plastic, limiting the generation of combustible gas, playing a role in heat insulation and oxygen isolation, and achieving a smoke suppression effect. At the same time, the hydrated metal oxide can also improve the dielectric properties of the matrix resin.
[0038] In some embodiments, the hydrated metal oxide flame retardant includes at least one of: aluminum hydroxide, magnesium hydroxide; and / or,
[0039] The coupling agent includes at least one of the following: borate, phosphate, titanate, aluminate, silane, stannate, zirconate.
[0040] In the embodiment of the present application, the hydrated metal oxide flame retardant can be a combination of one or more of aluminum hydroxide and magnesium hydroxide, and further, aluminum hydroxide can be selected. The coupling agent can be a combination of one or more of borate, phosphate, titanate, aluminate, silane, stannate, and zirconate, and further, borate and phosphate can be selected. The hydrated metal oxide treated has a better flame retardant effect, while reducing the use of flame retardants and inhibiting burning drips.
[0041] In some embodiments, the pretreated hydrated metal oxide flame retardant is obtained by pretreating the hydrated metal oxide flame retardant with a coupling agent, comprising:
[0042] The preparation method of the pretreated hydrated metal oxide flame retardant is as follows:
[0043] Under the condition of set temperature, the hydrated metal oxide flame retardant is stirred, and a coupling agent is added to the hydrated metal oxide flame retardant in stages to obtain a pretreated hydrated metal oxide flame retardant; wherein,
[0044] In the pretreated hydrated metal oxide flame retardant, the hydrated metal oxide flame retardant is 5 to 15 parts by weight, and the coupling agent is 1.5 to 3 parts by weight.
[0045] In the embodiment of the present application, in the pre-treated hydrated metal oxide flame retardant, the hydrated metal oxide flame retardant can be 5 to 15 parts by weight, and the coupling agent can be 1.5 to 3 parts, which can promote the coupling agent to improve the compatibility of the hydrated metal oxide flame retardant with the matrix resin SMA, and stably distribute in the matrix resin SMA, to achieve a good flame retardant effect, and reflect the good synergistic flame retardant effect of the coupling agent and the hydrated metal oxide flame retardant. Exemplarily, the hydrated metal oxide flame retardant can be 5 parts, 7 parts, 9 parts, 11 parts, 13 parts, 15 parts, etc., and the coupling agent is 1.5 parts, 2 parts, 2.5 parts, 3 parts, etc.
[0046] In some embodiments, the set temperature is 115°C to 120°C.
[0047] In the embodiment of the present application, the hydrated metal oxide flame retardant is stirred at high temperature so that the hydrated metal oxide flame retardant is fully dispersed and evenly dispersed, and the coupling agent is added to the hydrated metal oxide flame retardant in stages, which can promote the hydrated metal oxide flame retardant and the coupling agent to be fully mixed, so that the coupling agent and the aluminum hydroxide have a good interface connection effect, so that the hydrated metal oxide treated with the coupling agent can greatly improve the flame retardant properties of SMA and reduce the amount of flame retardant. Exemplarily, the above-mentioned set temperature can be 115°C, 116°C, 117°C, 118°C, 119°C, 120°C, etc. The above-mentioned stirring speed can be 1000r / min~1200r / min, and the coupling agent can be added in stages at least twice. Specifically, as one of the preparation methods of the pretreated hydrated metal oxide flame retardant, the method includes: according to weight, fully stirring aluminum hydroxide in a high-speed kneader at 115°C at 1000r / min, drying in an open air for 15 minutes, adding 60% and 40% of a coupling agent in two times, with an interval of 3 minutes in between, stirring for 4 minutes and then discharging to obtain a pretreated hydrated metal oxide flame retardant.
[0048] In some embodiments, the raw material components of the composite material further include: a filler, and the filler is obtained by surface treating aluminosilicate with a grafting agent.
[0049] In the embodiments of the present application, the surface of the aluminosilicate is treated with a grafting agent, which can improve the dispersibility of the aluminosilicate in the matrix resin SMA, and at the same time form a penetrating spatial network structure with the SMA matrix resin, thereby improving the impact resistance, electrical properties and heat resistance of the matrix, and having good dimensional stability at room and high temperatures.
[0050] In some embodiments, the grafting agent includes at least one of: maleic anhydride grafted polypropylene wax, aminosilane, aminoacetate; and / or,
[0051] The aluminosilicate includes at least one of the following: quartz powder, phlogopite powder, and muscovite powder.
[0052] In the embodiment of the present application, the grafting agent can be a combination of one or more of maleic anhydride grafted polypropylene wax, aminosilane, and aminoacetate, and further, maleic anhydride grafted polypropylene wax can be selected. The aluminosilicate can be a combination of one or more of quartz powder, phlogopite powder, and muscovite powder, and further, hard muscovite powder with good electrical insulation can be selected.
[0053] In some embodiments, the filler is obtained by surface treating aluminosilicate with a grafting agent, and includes:
[0054] The preparation method of the filler is as follows:
[0055] drying the aluminosilicate;
[0056] The dried aluminosilicate is mixed with a grafting agent to obtain a filler; wherein, in the filler, the aluminosilicate accounts for 10 to 20 parts by weight, and the grafting agent accounts for 5% to 6% of the weight of the aluminosilicate.
[0057] In the embodiment of the present application, the aluminosilicate has the function of improving the electrical properties of the SMA matrix resin. The aluminosilicate modified by the grafting agent can improve the dispersibility of the aluminosilicate in the matrix resin SMA, and at the same time form a through-space network structure with the SMA matrix resin, thereby further enhancing the electrical properties of the SMA composite material. The aluminosilicate can be 10 to 20 parts, and the grafting agent can be 5% to 6% by weight of the aluminosilicate, so that the aluminosilicate and the grafting agent can fully carry out a chemical grafting reaction. Exemplarily, the aluminosilicate can be 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, etc., and the grafting agent can be 5%, 5.5%, 6%, etc. by weight of the aluminosilicate. Specifically, the preparation method of one of the fillers includes: first putting mica powder into a high-speed mixing mixer, drying it at 115°C to 120°C for 1.5h to 2h, then adding maleic anhydride grafted polypropylene wax according to 5% of the weight of mica, stirring at 170 to 175°C for 40min to 45min to obtain the filler.
[0058] In some embodiments, the drying temperature is 115° C. to 120° C.; and / or,
[0059] The mixing temperature is 170°C to 175°C.
[0060] In the embodiment of the present application, the aluminosilicate is dried to remove moisture and improve the fluidity and mixing uniformity of the aluminosilicate. The aluminosilicate and the grafting agent are mixed at high temperature to further promote the full progress of the chemical grafting reaction. Exemplarily, the drying temperature can be 115°C, 116°C, 117°C, 118°C, 119°C, 120°C, etc., and the mixing temperature can be 170°C, 171°C, 172°C, 173°C, 174°C, 175°C, etc.
[0061] In summary, by pretreating the hydrated metal oxide flame retardant with a coupling agent and surface treating the aluminosilicate with a grafting agent, a stable spatial network structure of the SMA matrix can be formed, which effectively improves the volume resistivity and dielectric strength of the SMA material, and has excellent flame retardancy and smoke suppression. At the same time, due to the existence of the spatial network structure, the SMA matrix has good mechanical properties and heat resistance.
[0062] In some embodiments, the raw material components of the composite material further include: a second matrix resin and an auxiliary agent.
[0063] In the embodiment of the present application, the second matrix resin can improve the impact resistance of the composite material. At the same time, as the matrix resin of the functional masterbatch, the second matrix resin can include ABS (acrylonitrile-butadiene-styrene copolymer) or styrene resin, wherein the rubber powder (butadiene) content in ABS can be 55wt% to 70wt%; further, the rubber powder content in ABS can be 65wt%; styrene resin can include HIPS (high impact polystyrene), AS (acrylonitrile-styrene copolymer), etc. The auxiliary agent can include at least one of the following: an antioxidant, an impact modifier, a lubricant, and a reinforcing agent. Among them, the antioxidant can improve the processing and antioxidant effect of the composite material; the impact modifier improves the impact resistance of the composite material; the lubricant can improve the processing performance of the composite material; the reinforcing agent can improve the mechanical properties of the composite material.
[0064] Further, the content of maleic anhydride in SMA can be 10wt% to 25wt%; further, the content of maleic anhydride can be 15wt% to 25wt%. The second matrix resin can include ABS (acrylonitrile-butadiene-styrene copolymer) or styrene resin, wherein the content of rubber powder (butadiene) in ABS can be 55wt% to 70wt%; further, the content of rubber powder in ABS can be 65wt%; styrene resin can include HIPS (high impact polystyrene), AS (acrylonitrile-styrene copolymer), etc. The antioxidant can be hindered phenols, further, it can be 4,4'-thiobis(6-tert-butyl-3-methylphenol), 2,2'-thiobis(6-tert-butyl-4-methylphenol), antioxidant 2246-S, etc. The impact modifier is one or more of SBS (styrene-butadiene-styrene block copolymer), SEBS (hydrogenated styrene-butadiene-styrene triblock copolymer), ABS (acrylonitrile-styrene-butadiene copolymer), EPR (ethylene propylene rubber), BR (cis-butadiene rubber), SBR (styrene-butadiene rubber); further, the impact modifier can be SBS, and SBS uses a star structure. The lubricant can be one or more of butyl stearate, paraffin oil, liquid polybutene, and zinc stearate; further, the lubricant can be a mixture of butyl stearate and zinc stearate. The reinforcing agent can be glass fiber, and further, the reinforcing agent can be chopped glass fiber with a diameter of 9μm to 13μm and a length of 6mm; further, a diameter of 11μm and a length of 6mm. The raw material components in the composite material are reasonably designed to ensure the performance of the composite material.
[0065] One of the SMA composite materials includes: a first matrix resin, a second matrix resin, an antioxidant, an impact modifier, a lubricant and a reinforcing agent, as well as the above-mentioned pretreated hydrated metal oxide flame retardant and filler; wherein, in parts by weight, the first matrix resin can be 60 to 75 parts, the second matrix resin can be 10 to 15 parts, the antioxidant can be 0.5 to 1.5 parts, the impact modifier can be 10 to 20 parts, the lubricant can be 1 to 2 parts, and the reinforcing agent can be 10 to 25 parts.
[0066] A method for preparing a composite material based on styrene-maleic anhydride copolymer, Figure 1 A schematic diagram of a process for preparing a composite material based on styrene-maleic anhydride copolymer provided in an embodiment of the present application; see Figure 1, including: S1, pre-treating a hydrated metal oxide flame retardant with a coupling agent to obtain a pre-treated hydrated metal oxide flame retardant; S2, surface-treating aluminosilicate with a grafting agent to obtain a filler; S3, first mixing a base resin containing a styrene-maleic anhydride copolymer with an auxiliary agent, and then performing a first melt blending to obtain a mixed material; S4, second mixing the pre-treated hydrated metal oxide flame retardant, the filler and the mixed material, and then performing a second melt blending to obtain a composite material based on styrene-maleic anhydride copolymer.
[0067] Furthermore, S3 specifically includes: mixing the SMA-containing matrix resin and the additive in a high-pressure mixer in parts by weight, and then melt-blending them in a twin-screw extruder, and obtaining a mixed material after drawing, cooling, drying and pelletizing; wherein the twin-screw extruder in S3 is a co-rotating twin-screw extruder, the twin-screw extruder cooling device adopts water cooling, the screw diameter of the twin-screw extruder is Φ21.7, the aspect ratio is 40 / 1, the temperature range is 230-250°C, wherein the first zone is 230°C, the second zone is 235°C, and the third zone is 240°C. , the screw speed is 500rpm; S4 specifically includes: the pre-treated hydrated metal oxide flame retardant, filler and mixed material are mixed evenly, and then enter the extruder through the feeding port of the twin-screw extruder for melt blending, and at the same time, the reinforcing agent is transported into the extruder screw through the side feeding port at the rear end of the screw, and further melt blended with the pre-treated hydrated metal oxide flame retardant, filler and mixed material, and then after drawing, cooling, drying and pelletizing, a composite material based on styrene-maleic anhydride copolymer (SMA composite material) is obtained. Among them, the twin-screw extruder in S4 is a co-rotating twin-screw extruder, the twin-screw extruder cooling device adopts water cooling, the screw diameter of the twin-screw extruder is Φ21.7, the aspect ratio is 40 / 1, the temperature range is 250-270℃, the first zone is 250℃, the second zone is 255℃, the third zone is 260℃, and the screw speed is 500rpm.
[0068] In a second aspect, the present application provides an application of a composite material based on styrene-maleic anhydride copolymer as described in any embodiment of the first aspect in a new energy vehicle.
[0069] In the embodiments of the present application, the composite material based on styrene-maleic anhydride copolymer meets the following properties: flame retardancy reaches V0, relative tracking index reaches 600V, dielectric strength ≥60kV / mm, volume resistivity ≥10 16 Ohm·m, tensile strength ≥80MPa, simply supported beam notched impact strength ≥9KJ / m 2Therefore, the composite material based on styrene-maleic anhydride copolymer not only has the same excellent performance in mechanical properties, but also has good electrical properties and flame retardant properties, making it not only suitable for ordinary new energy vehicle interior and exterior parts, but also for new energy vehicle three-electric system component materials.
[0070] The application of the composite material based on styrene-maleic anhydride copolymer in new energy vehicles is achieved based on the above-mentioned composite material based on styrene-maleic anhydride copolymer. The specific raw materials of the composite material based on styrene-maleic anhydride copolymer can refer to the above-mentioned embodiment. Since the composite material based on styrene-maleic anhydride copolymer adopts part or all of the technical solutions of the above-mentioned embodiment, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be repeated here one by one.
[0071] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0072] The raw materials used in the examples of the present application are from the following sources: SMA resin: MA content 22.5%, purchased from Crayville, USA, brand SMA 3000; ABS resin: rubber content 60-65%, Shandong Wanda, brand WD-132; antioxidant: purity 99%, Mitsui Chemicals, model antioxidant 300; SBS: Kraton, brand D1102 JSZ; SBR: Kumho, South Korea, brand 1502; Butyl stearate: purity 99%, Shandong Shouhua Chemical; Zinc stearate: purity 99%, Shandong Xinghai Chemical, model XH-159; Paraffin oil: Shandong Zhuyou Lubrication Technology Co., Ltd.; Muscovite powder: 1000 mesh, Donghai County Fucai Mineral Products Co., Ltd.; Maleic anhydride grafted polypropylene wax: Clariant, model PPWAX-MAH; Glass fiber: diameter 11μm, length 6mm, Shandong Tonghui Glass Fiber Co., Ltd.; Aluminum hydroxide: purity 99%, 1200 mesh, Chalco; Borate: purchased from Qingdao Rongyao Rubber and Plastic New Materials Co., Ltd., brand PRA-20; Phosphate: purity 95%, Jiangsu Hai'an Petrochemical Plant, specification MOA-3P; Titanate: purity 99.9%, Japan Soda, model B-1.
[0073] A method for preparing a composite material based on styrene-maleic anhydride copolymer, specifically comprising:
[0074] Step 1: first, by weight, put mica powder into a high-speed mixing mixer, dry it at 120° C. for 1.5 hours, then add maleic anhydride grafted polypropylene wax according to 5% of the amount of mica, stir at 170° C. for 40 minutes, and cool to room temperature to obtain a pretreated hydrated metal oxide flame retardant;
[0075] Step 2: According to the weight, aluminum hydroxide is fully stirred in a high-speed kneader at 115°C, dried in an open oven for 15 minutes, and 60% and 40% of the coupling agent are added twice, respectively, with an interval of 3 minutes in between, and the material is discharged after stirring for 4 minutes to obtain a filler;
[0076] Step 3: SMA, ABS, antioxidant, impact modifier, lubricant and filler are mixed uniformly in a high mixer according to weight, and then melt-blended by a twin-screw extruder, and then subjected to drawing, cooling, drying and pelletizing to obtain a mixed material; wherein the twin-screw extruder is a co-rotating twin-screw extruder, the twin-screw extruder cooling device adopts a water cooling method, the screw diameter of the twin-screw extruder is Φ21.7, the aspect ratio is 40 / 1, the temperature range is 230-250°C, wherein the first zone is 230°C, the second zone is 235°C, the third zone is 240°C, and the screw speed is 500rpm;
[0077] Step 4: The pre-treated hydrated metal oxide flame retardant, filler and mixed material are mixed evenly, and then enter the extruder through the feeding port of the twin-screw extruder for melt blending, and at the same time, the glass fiber is transported into the extruder screw through the side feeding port at the rear end of the screw, and further melt blended with the pre-treated hydrated metal oxide flame retardant, filler and mixed material, and then after drawing, cooling, drying and pelletizing, a composite material based on styrene-maleic anhydride copolymer is obtained. Among them, the twin-screw extruder is a co-rotating twin-screw extruder, the twin-screw extruder cooling device adopts water cooling, the screw diameter of the twin-screw extruder is Φ21.7, the aspect ratio is 40 / 1, the temperature range is 250-270°C, the first zone is 250°C, the second zone is 255°C, the third zone is 260°C, and the screw speed is 500rpm. For details, please refer to the weight parts of each raw material of the composite materials based on styrene-maleic anhydride copolymer in Examples 1 to 8 shown in Table 1; the weight parts of each raw material of the composite materials based on styrene-maleic anhydride copolymer in Examples 9 to 16 shown in Table 2; and the weight parts of each raw material of the composite materials based on styrene-maleic anhydride copolymer in Comparative Examples 1 to 6 shown in Table 6.
[0078] Table 1 Weight parts of raw materials of composite materials based on styrene-maleic anhydride copolymer in Examples 1 to 8
[0079]
[0080] Table 2 Weight parts of raw materials of composite materials based on styrene-maleic anhydride copolymer in Examples 9 to 16
[0081]
[0082]
[0083] Table 3 Weight parts of raw materials of composite materials based on styrene-maleic anhydride copolymer in Comparative Examples 1 to 6
[0084]
[0085] The mechanical properties, electrical properties and flame retardant properties of Examples 1 to 16 and Comparative Examples 1 to 6 were tested. For details, please refer to the performance test results of the composite materials based on styrene-maleic anhydride copolymer of Examples 1 to 8 shown in Table 4; the performance test results of the composite materials based on styrene-maleic anhydride copolymer of Examples 9 to 16 shown in Table 5; and the performance test results of the composite materials based on styrene-maleic anhydride copolymer of Comparative Examples 1 to 6 shown in Table 6.
[0086] The following test methods are used to illustrate the material properties disclosed in the examples of the present application: (1) tensile strength, refer to ISO527 standard, tensile rate 5 mm / min; (2) elongation at break, refer to ISO 527 standard, tensile rate 5 mm / min; (3) simply supported beam notched impact strength: refer to ISO 179-1 standard; (4) dielectric strength, refer to IEC 60243-1 standard; (5) volume resistivity: refer to IEC 62631-3-1 standard; (6) comparative tracking index CTI: refer to IEC 60112 standard; (7) flame retardancy: refer to UL94 standard, thickness 1.5 mm.
[0087] Table 4 Performance test results of composite materials based on styrene-maleic anhydride copolymer in Examples 1 to 8
[0088]
[0089] Table 5 Performance test results of composite materials based on styrene-maleic anhydride copolymer in Examples 9 to 16
[0090]
[0091]
[0092] Table 6 Performance test results of composite materials based on styrene-maleic anhydride copolymer in Comparative Examples 1 to 6
[0093]
[0094] As shown in Tables 1 to 6, in Examples 1 to 16, mica powder significantly improves the electrical properties of the composite material, mica powder treated with maleic anhydride grafted polypropylene wax has better electrical properties, aluminum hydroxide significantly improves the flame retardant properties of the material, and aluminum hydroxide treated with a coupling agent has better flame retardant properties. Specifically, as shown in Examples 5 and 13, the impact modifier SBS has a better toughening effect; as shown in Examples 5 and 14, different lubricants have little effect on the performance of the composite material, but butyl stearate and zinc stearate are the best solutions; as shown in Examples 5, 15 and 16, different coupling agents have little effect on the performance of the composite material, but borate is the best solution. In Comparative Example 1, no pre-treatment flame retardant aluminum hydroxide was added, and the flame retardant performance was worse than that of the embodiment; in Comparative Example 2, the content of coupling agent borate ester added was too low, and the content of flame retardant aluminum hydroxide was too low, and the content of pre-treatment flame retardant was low, and the flame retardant performance of the final composite material was worse than that of the embodiment, and did not meet the V-0 requirement; in Comparative Example 3, the content of flame retardant aluminum hydroxide added was too high, and the flame retardant performance of the final composite material met the standard, but the toughness (elongation at break) of the material deteriorated, and the impact strength was only 7.6 KJ / m 2 ; In Comparative Example 4, a flame retardant was added but no coupling treatment was performed, and the flame retardant properties of the composite material met the standard, but the mechanical properties of the composite material were significantly reduced, and the electrical properties were also reduced; in Comparative Example 5, no filler was added, and the electrical properties of the composite material were poor, the dielectric strength was only 35kV / mm, and the relative tracking index CTI was only 300V; In Comparative Example 6, the mica powder added was not treated with maleic anhydride grafted polypropylene wax, and the electrical properties of the composite material were significantly improved, but the tensile strength, notched impact strength and dielectric strength were reduced to a certain extent. Maleic anhydride grafted polypropylene wax treatment can significantly improve the comprehensive performance of the composite material.
[0095] Therefore, it can be seen from the test results of the above Examples 1 to 16 that the SMA composite materials provided in the embodiments of the present application have excellent performance in mechanical properties, electrical properties and flame retardant properties. Compared with traditional SMA materials, the strength and toughness are almost unaffected, and it has better flame retardancy, dielectric strength and relative tracking index, and is fully suitable for the three-electric system of new energy vehicles.
[0096] One or more technical solutions in the embodiments of the present application also have at least the following technical effects or advantages:
[0097] (1) The hydrated metal oxide flame retardant is pretreated with a coupling agent, so that the hydrated metal oxide flame retardant and the coupling agent have a good interface connection effect, thereby improving the compatibility of the hydrated metal oxide flame retardant with the matrix resin styrene-maleic anhydride copolymer, and the dispersibility of the hydrated metal oxide flame retardant in the matrix resin styrene-maleic anhydride copolymer, so that the pretreated hydrated metal oxide flame retardant is stably and uniformly dispersed in the matrix resin styrene-maleic anhydride copolymer, and the coupling agent cooperates with the hydrated metal oxide flame retardant to improve the flame retardant properties of the composite material of styrene-maleic anhydride copolymer;
[0098] (2) The surface treatment of aluminosilicate by a grafting agent can improve the dispersibility of aluminosilicate in the matrix resin SMA, and at the same time form a through-space network structure with the SMA matrix resin, thereby further enhancing the electrical properties of the SMA composite material;
[0099] (3) The synergistic effect of pre-treating the hydrated metal oxide flame retardant with a coupling agent and surface-treating the aluminosilicate with a grafting agent can form a stable spatial network structure of the SMA matrix, which effectively improves the volume resistivity and dielectric strength of the SMA material, and has excellent flame retardancy and smoke suppression. At the same time, due to the existence of the spatial network structure, the SMA matrix has good mechanical properties and heat resistance.
[0100] (4) Compared with conventional SMA reinforced and toughened materials, the SMA composite material provided in the embodiments of the present application not only has the same excellent performance in mechanical properties, but also has good electrical properties and flame retardant properties, so that it can be used not only for ordinary new energy vehicle interior and exterior parts, but also for new energy vehicle three-electric system component materials.
[0101] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A composite material based on styrene-maleic anhydride copolymer, characterized in that: The raw material components of the composite material include: a first base resin and a pretreated hydrated metal oxide flame retardant; The first base resin includes styrene-maleic anhydride copolymer, and the pretreated hydrated metal oxide flame retardant is obtained by pretreating the hydrated metal oxide flame retardant with a coupling agent.
2. The composite material according to claim 1, characterized in that The hydrated metal oxide flame retardant comprises at least one of the following: aluminum hydroxide, magnesium hydroxide; and / or, The coupling agent includes at least one of the following: borate, phosphate, titanate, aluminate, silane, stannate, zirconate.
3. The composite material according to claim 1 or 2, characterized in that: The pretreated hydrated metal oxide flame retardant is obtained by pretreating the hydrated metal oxide flame retardant with a coupling agent, and comprises: The preparation method of the pretreated hydrated metal oxide flame retardant is as follows: Under the condition of set temperature, the hydrated metal oxide flame retardant is stirred, and a coupling agent is added to the hydrated metal oxide flame retardant in stages to obtain a pretreated hydrated metal oxide flame retardant; wherein, In the pretreated hydrated metal oxide flame retardant, the hydrated metal oxide flame retardant is 5 to 15 parts by weight, and the coupling agent is 1.5 to 3 parts by weight.
4. The composite material according to claim 3, characterized in that The set temperature is 115°C to 120°C.
5. The composite material according to claim 1, characterized in that The raw material components of the composite material also include: a filler, and the filler is obtained by surface treating aluminosilicate with a grafting agent.
6. The composite material according to claim 4, characterized in that The grafting agent comprises at least one of the following: maleic anhydride grafted polypropylene wax, aminosilane, aminoacetate; and / or, The aluminosilicate includes at least one of the following: quartz powder, phlogopite powder, and muscovite powder.
7. The composite material according to claim 4 or 5, characterized in that: The filler is obtained by surface treating aluminosilicate with a grafting agent, and includes: The preparation method of the filler is as follows: drying the aluminosilicate; The dried aluminosilicate is mixed with a grafting agent to obtain a filler; wherein, in the filler, the aluminosilicate accounts for 10 to 20 parts by weight, and the grafting agent accounts for 5% to 6% of the weight of the aluminosilicate.
8. The composite material according to claim 6, characterized in that The drying temperature is 115°C to 120°C; and / or, The mixing temperature is 170°C to 175°C.
9. The composite material according to claim 1, characterized in that The raw material components of the composite material also include: a second matrix resin and an auxiliary agent.
10. Use of the composite material based on styrene-maleic anhydride copolymer according to any one of claims 1 to 9 in new energy vehicles.