Degradable high-flexibility hydrophobic packaging material and preparation method thereof

Through the blending of polylactic acid with modified filler and nanofiber colloidal solution, combined with the use of modified treatment solution, the problem of insufficient toughness and hydrophobicity of polylactic acid materials is solved, and a packaging with high flexibility and hydrophobicity is prepared. Material, suitable for cosmetics and pharmaceutical packaging.

CN118931134AInactive Publication Date: 2024-11-12GUANGZHOU LAIDU BRAND MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411180507.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In actual applications, polylactic acid packaging materials have problems such as insufficient toughness, strong hygroscopicity, poor interface compatibility and insufficient hydrophobic performance, which limits their wider application.

Method used

By blending polylactic acid with modified filler and processing with nanofiber colloidal solution and modification treatment solution, a firm interface bonding and complex network structure is formed to improve the flexibility and tensile resistance of the material, while at the same time, the modification is carried out through The treatment liquid enhances the hydrophobic properties of the material.

Benefits of technology

The prepared packaging material has excellent flexibility and hydrophobicity, and has improved flexural strength, tensile strength and tensile elongation at break, and has a low water absorption rate of 72 hours. It is suitable as a degradable high-performance packaging material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012002560000111
    Figure BDA0005012002560000111
  • Figure BDA0005012002560000121
    Figure BDA0005012002560000121
Patent Text Reader

Abstract

The invention relates to a degradable high-flexibility hydrophobic packaging material and a preparation method thereof, and belongs to the technical field of packaging materials. The preparation method of the packaging material comprises the following steps: mixing the polylactic acid and the modified filler, and treating to obtain a mixture; mixing the mixture, the nanofiber colloidal solution and the modified treatment liquid, and treating to obtain a solid material; and finally, mixing the solid material and an antioxidant, and performing melt extrusion to obtain the degradable high-flexibility hydrophobic packaging material. The polylactic acid and the modified filler are blended to form firm interface bonding, then molecular interaction and physical winding are formed by means of a nanofiber colloidal solution, the flexibility and tensile property of the material are further improved, and finally the hydrophobic property from the interior of molecules to the surface is improved under the action of a modification treatment solution. The prepared packaging material has excellent flexibility and hydrophobicity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of packaging materials and relates to a degradable high-flexibility hydrophobic packaging material and a preparation method thereof. Background Art

[0002] With the development of the times, people's environmental awareness has been continuously strengthened and deepened, and the demand for degradable packaging materials has also shown an increasing and more urgent trend. In the field of cosmetics and pharmaceuticals, the selection of packaging materials is crucial. Traditional packaging materials used in the past, such as common plastics and glass, often remain in the environment for a long time after being discarded, and are difficult to naturally decompose, causing many problems to the ecological environment. The emergence of polylactic acid materials has brought new opportunities for change in the packaging of cosmetics and pharmaceuticals. Its excellent degradable properties enable packaging products such as cosmetic packaging capsules and pharmaceutical capsules made of polylactic acid to be gradually decomposed by microorganisms in the natural environment after completing their mission, thereby minimizing pollution and damage to the environment.

[0003] However, based on the properties of polylactic acid, there are still some deficiencies in its practical application. For example, a variety of toughening agents or other fillers are usually added during the preparation to improve the overall toughness of the polylactic acid material. However, polylactic acid, as a weakly polar polymer, is easy to affect the interfacial compatibility between materials when multiple materials are mixed, resulting in reduced internal material bonding, making the material prone to cracking, and affecting the overall mechanical properties of the material. In addition, polylactic acid itself is hygroscopic and is easy to absorb moisture when used as a packaging material, affecting the preservation of the packaging contents and the service life of the packaging material. The deficiencies in flexibility and hydrophobicity limit its wider application. Summary of the invention

[0004] The object of the present invention is to provide a degradable, highly flexible, hydrophobic packaging material and a preparation method thereof. The present invention blends polylactic acid with a modified filler to form a firm interface bond, and then uses a nanofiber colloidal solution to form molecular action and physical entanglement to further improve the flexibility and tensile strength of the material. Finally, under the action of a modified treatment liquid, the hydrophobic properties are improved from the inside of the molecule to the surface. The prepared packaging material has excellent flexibility and hydrophobicity.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing a degradable high-flexibility hydrophobic packaging material, the preparation method comprising the following steps:

[0007] (1) mixing polylactic acid, modified filler and deionized water, ball milling and passing through a 80-200 mesh sieve to obtain a mixture;

[0008] (2) mixing the mixed material, the nanofiber colloid solution and the modified treatment liquid, ultrasonicating, centrifuging, filtering, washing with deionized water and drying to obtain a solid material;

[0009] (3) The solid material and the antioxidant are mixed and melted in a twin-screw extruder, extruded after stirring, and cooled to obtain a degradable, highly flexible, hydrophobic packaging material.

[0010] As a preferred technical solution of the present invention, the mass ratio of polylactic acid, modified filler and deionized water in step (1) is 5.26-7.3:1.14-1.8:8-10; the molecular weight of the polylactic acid is 120000-180000; the parameters of the ball milling step are: ball milling speed is 100-300rmp, and ball milling time is 20-30min.

[0011] As a preferred technical solution of the present invention, the preparation method of the modified filler is:

[0012] The filler is crushed into 100-200 mesh, soaked in 1-3 mol / L hydrochloric acid solution for 2-4 hours, filtered, and the obtained solid A is washed with deionized water, and then dried in a 90°C oven for 3-5 hours to obtain a dry product; the dry product, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and anhydrous ethanol are added to a reactor, stirred and mixed, and then filtered. The obtained solid B is washed with anhydrous ethanol and then dried in a 60°C oven for 6-8 hours to obtain a modified filler.

[0013] As a preferred technical solution of the present invention, the filler is composed of clay mineral and talc in a mass ratio of 6.8-8.1:0.8-1.7; the clay mineral is selected from one or more of montmorillonite, kaolin and illite; the mass ratio of the dried product, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and anhydrous ethanol is 5.2-8.6:0.7-1.1:18-30; the filtration uses a 200-300 mesh filter cloth; the parameters of the reactor are: temperature of 60-70°C, rotation speed of 300-500rmp, and time of 2.5-4.5h.

[0014] As a preferred technical solution of the present invention, the mass of the nanofiber colloidal solution in the step (2) accounts for 10-12wt% of the mixture, and the mass of the modified treatment liquid accounts for 5-8wt% of the mixture; the parameters of the ultrasonic treatment are: ultrasonic frequency is 20-60kHz, ultrasonic power is 100-300W, ultrasonic temperature is 40-60℃, and ultrasonic time is 40-60min; the parameters of the centrifugal treatment are: centrifugal speed is 3000-5000rmp, and centrifugal time is 10-20min.

[0015] As a preferred technical solution of the present invention, the preparation method of the nanofiber colloid solution is:

[0016] Chlorella powder with a particle size of 100-200 mesh is added to deionized water, and stirred at a speed of 400-500 rpm for 1-2 hours to obtain a suspension with a mass concentration of 1-3 wt%. The suspension is subjected to high-pressure homogenization, centrifugation, and the supernatant is collected and dialyzed to obtain a nanofiber colloidal solution.

[0017] As a preferred technical solution of the present invention, the parameters of the high-pressure homogenization treatment are: homogenization pressure of 80-100MPa, number of homogenizations of 4 times, homogenization time of 5min, and each homogenization interval of 2min; the parameters of the centrifugal treatment are: centrifugal speed of 6000-10000rmp, and centrifugal time of 10-20min; the steps of the dialysis treatment are: pouring the supernatant into a dialysis bag with a molecular weight cutoff of 4000-6000D, placing the dialysis bag in a container containing 2L of deionized water, replacing the deionized water every 4h, and the dialysis cycle is 24h.

[0018] As a preferred technical solution of the present invention, the preparation method of the modified treatment liquid is:

[0019] Perfluorooctyltriethoxysilane, surfactant, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, potassium persulfate and ethanol solution are mixed in a mass ratio of 1.4-1.8:0.52-0.7:0.25-0.35:0.07-0.11:9-12, and stirred at a speed of 600-800 rpm for 2-3 hours to obtain a modified treatment solution.

[0020] As a preferred technical solution of the present invention, the surfactant is selected from one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and Tween-80; the mass concentration of the ethanol solution is 70-80wt%.

[0021] As a preferred technical solution of the present invention, the mass of the antioxidant in the step (3) accounts for 0.1-0.5wt% of the solid material, and the antioxidant is selected from one or more of antioxidant 1010 and antioxidant 168; the temperature of the melting step in the step (3) is 150-180°C; the stirring speed in the step (3) is 100-500rmp.

[0022] Beneficial effects of the present invention:

[0023] (1) In the present invention, clay minerals and talc are modified to obtain modified fillers. Talc has a unique layered structure and active sites exist on its surface. When talc is combined with clay minerals, these active sites can adsorb clay and play a role of spacing and lubrication in clay particles, so that clay molecules can be orderly and uniformly dispersed during subsequent processing, interact with the epoxy group of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and then chemically bond with the end group or side chain of the polylactic acid molecule to form a strong interface bond. This good interface bond effectively transmits stress at the molecular level and can prevent the expansion of cracks, thereby improving the strength and toughness of the material.

[0024] (2) The present invention uses Chlorella powder as a raw material to prepare a nanofiber colloidal solution, which is cheaper and easier to obtain than other nanofiber materials. The nanofibers prepared from Chlorella powder have a high specific surface area and aspect ratio, and can form a complex network structure in the material. Secondly, the surface of the nanofibers is rich in functional groups such as hydroxyl and carboxyl groups, which can form hydrogen bonds or produce physical entanglement with the polylactic acid molecular chains. This entanglement restricts the free movement of the polylactic acid molecular chains and plays a role of internal plasticization. When stretched by external force, the nanofibers can effectively disperse and absorb energy and organize the rapid expansion of cracks, thereby improving the flexibility and tensile resistance of the material.

[0025] (3) The perfluorocarbon chain in the perfluorooctyltriethoxysilane in the modified treatment liquid of the present invention has extremely low surface energy and tends to migrate to the surface of the material during ultrasonic treatment, and is enriched on the surface of the material to form a hydrophobic layer, which makes it difficult for water molecules to adhere to and penetrate the surface of the material, giving the material excellent hydrophobic properties; the epoxy group in γ-(2,3-epoxypropoxy)propyltrimethoxysilane can interact with the active groups on the polylactic acid molecular chain, introduce the silicon-containing hydrophobic chain segment into the molecular structure of the polylactic acid, and realize the improvement of the hydrophobic performance from the inside of the molecule to the surface, thereby synergistically exerting the hydrophobic effect. DETAILED DESCRIPTION

[0026] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0027] Example 1

[0028] A method for preparing a degradable, highly flexible, hydrophobic packaging material. The preparation method of this embodiment comprises the following steps:

[0029] (1) mixing polylactic acid, modified filler and deionized water, ball milling and passing through an 80-mesh sieve to obtain a mixture;

[0030] (2) mixing the mixed material, the nanofiber colloid solution and the modified treatment liquid, ultrasonicating, centrifuging, filtering, washing with deionized water and drying to obtain a solid material;

[0031] (3) The solid material and the antioxidant are mixed and melted in a twin-screw extruder, extruded after stirring, and cooled to obtain a degradable, highly flexible, hydrophobic packaging material.

[0032] The mass ratio of polylactic acid, modified filler and deionized water in step (1) of this embodiment is 5.26:1.14:8; the molecular weight of the polylactic acid of this embodiment is 120,000; the parameters of the ball milling step of this embodiment are: ball milling speed is 100 rpm, and ball milling time is 20 min.

[0033] The preparation method of the modified filler of this embodiment is:

[0034] The filler was crushed into 100 mesh, soaked in 1 mol / L hydrochloric acid solution for 2 hours, filtered, and the obtained solid A was washed with deionized water, and then dried in an oven at 90°C for 3 hours to obtain a dry product; the dry product, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and anhydrous ethanol were added to a reactor, stirred and mixed, and then filtered. The obtained solid B was washed with anhydrous ethanol and then dried in an oven at 60°C for 6 hours to obtain a modified filler.

[0035] The filler of this embodiment is composed of clay mineral and talc in a mass ratio of 6.8:0.8; the clay mineral of this embodiment is kaolin; the mass ratio of the dried product, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and anhydrous ethanol in this embodiment is 5.2:0.7:18; the filtration in this embodiment uses a 200-mesh filter cloth; the parameters of the reactor in this embodiment are: temperature of 60°C, rotation speed of 300rmp, and time of 2.5h.

[0036] The mass of the nanofiber colloidal solution in step (2) of this embodiment accounts for 10wt% of the mixture, and the mass of the modified treatment liquid of this embodiment accounts for 5wt% of the mixture; the parameters of the ultrasonic treatment of this embodiment are: ultrasonic frequency is 20kHz, ultrasonic power is 100W, ultrasonic temperature is 40℃, and ultrasonic time is 40min; the parameters of the centrifugal treatment of this embodiment are: centrifugal speed is 3000rmp, and centrifugal time is 10min.

[0037] The preparation method of the nanofiber colloid solution of this embodiment is:

[0038] Chlorella powder with a particle size of 100 meshes was added to deionized water and stirred at a speed of 400 rpm for 1 hour to obtain a suspension with a mass concentration of 1 wt%. The suspension was subjected to high-pressure homogenization, centrifugation, and the supernatant was collected and dialyzed to obtain a nanofiber colloidal solution.

[0039] The parameters of the high-pressure homogenization treatment in this embodiment are: the homogenization pressure is 80MPa, the number of homogenizations is 4 times, the homogenization time is 5min, and the interval between each homogenization is 2min; the parameters of the centrifugal treatment in this embodiment are: the centrifugal speed is 6000rmp, and the centrifugal time is 10min; the steps of the dialysis treatment in this embodiment are: pouring the supernatant into a dialysis bag with a molecular weight cutoff of 4000D, placing the dialysis bag in a container containing 2L of deionized water, replacing the deionized water every 4h, and the dialysis cycle is 24h.

[0040] The preparation method of the modified treatment liquid of this embodiment is:

[0041] Perfluorooctyltriethoxysilane, surfactant, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, potassium persulfate and ethanol solution were mixed in a mass ratio of 1.4:0.52:0.25:0.07:9, and stirred at a speed of 600 rpm for 2 hours to obtain a modified treatment solution.

[0042] The surfactant of this embodiment is sodium dodecylbenzene sulfonate; the mass concentration of the ethanol solution of this embodiment is 70wt%.

[0043] The mass of the antioxidant in step (3) of this embodiment accounts for 0.1wt% of the solid material, and the antioxidant in this embodiment is antioxidant 1010; the temperature of the melting step in step (3) of this embodiment is 150°C; the stirring speed in step (3) of this embodiment is 100rmp.

[0044] Example 2

[0045] A method for preparing a degradable, highly flexible, hydrophobic packaging material. The preparation method of this embodiment comprises the following steps:

[0046] (1) mixing polylactic acid, modified filler and deionized water, ball milling and passing through a 200-mesh sieve to obtain a mixture;

[0047] (2) mixing the mixed material, the nanofiber colloid solution and the modified treatment liquid, ultrasonicating, centrifuging, filtering, washing with deionized water and drying to obtain a solid material;

[0048] (3) The solid material and the antioxidant are mixed and melted in a twin-screw extruder, extruded after stirring, and cooled to obtain a degradable, highly flexible, hydrophobic packaging material.

[0049] The mass ratio of polylactic acid, modified filler and deionized water in step (1) of this embodiment is 7.3:1.8:10; the molecular weight of the polylactic acid of this embodiment is 180000; the parameters of the ball milling step of this embodiment are: ball milling speed is 300rmp, and ball milling time is 30min.

[0050] The preparation method of the modified filler of this embodiment is:

[0051] The filler was crushed into 200 mesh, soaked in a 3 mol / L hydrochloric acid solution for 4 hours, filtered, and the obtained solid A was washed with deionized water, and then dried in an oven at 90°C for 5 hours to obtain a dry product; the dry product, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and anhydrous ethanol were added to a reactor, stirred and mixed, and then filtered. The obtained solid B was washed with anhydrous ethanol and then dried in an oven at 60°C for 8 hours to obtain a modified filler.

[0052] The filler of this embodiment is composed of clay mineral and talc in a mass ratio of 8.1:1.7; the clay mineral of this embodiment is kaolin; the mass ratio of the dried product, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and anhydrous ethanol in this embodiment is 8.6:1.1:30; the filtration in this embodiment uses a 300-mesh filter cloth; the parameters of the reactor in this embodiment are: temperature of 70°C, rotation speed of 500rmp, and time of 4.5h.

[0053] The mass of the nanofiber colloidal solution in step (2) of this embodiment accounts for 12wt% of the mixture, and the mass of the modified treatment liquid of this embodiment accounts for 8wt% of the mixture; the parameters of the ultrasonic treatment of this embodiment are: ultrasonic frequency is 60kHz, ultrasonic power is 300W, ultrasonic temperature is 60℃, and ultrasonic time is 60min; the parameters of the centrifugal treatment of this embodiment are: centrifugal speed is 5000rmp, and centrifugal time is 20min.

[0054] The preparation method of the nanofiber colloid solution of this embodiment is:

[0055] Chlorella powder with a particle size of 200 meshes was added to deionized water and stirred at a speed of 500 rpm for 2 hours to obtain a suspension with a mass concentration of 3 wt%. The suspension was homogenized under high pressure, centrifuged, and the supernatant was collected and dialyzed to obtain a nanofiber colloidal solution.

[0056] The parameters of the high-pressure homogenization treatment in this embodiment are: homogenization pressure of 100 MPa, number of homogenizations of 4 times, homogenization time of 5 min, and an interval of 2 min between each homogenization; the parameters of the centrifugal treatment in this embodiment are: centrifugal speed of 10000 rpm, and centrifugal time of 20 min; the steps of the dialysis treatment in this embodiment are: pouring the supernatant into a dialysis bag with a molecular weight cutoff of 6000D, placing the dialysis bag in a container containing 2L of deionized water, replacing the deionized water every 4 hours, and the dialysis cycle is 24 hours.

[0057] The preparation method of the modified treatment liquid of this embodiment is:

[0058] Perfluorooctyltriethoxysilane, surfactant, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, potassium persulfate and ethanol solution were mixed in a mass ratio of 1.8:0.7:0.35:0.11:12, and stirred at a speed of 800 rpm for 3 hours to obtain a modified treatment solution.

[0059] The surfactant of this embodiment is sodium dodecylbenzene sulfonate; the mass concentration of the ethanol solution of this embodiment is 80wt%.

[0060] The mass of the antioxidant in step (3) of this embodiment accounts for 0.5wt% of the solid material, and the antioxidant in this embodiment is antioxidant 1010; the temperature of the melting step in step (3) of this embodiment is 180°C; the stirring speed in step (3) of this embodiment is 500rmp.

[0061] Example 3

[0062] A method for preparing a degradable, highly flexible, hydrophobic packaging material. The preparation method of this embodiment comprises the following steps:

[0063] (1) mixing polylactic acid, modified filler and deionized water, ball milling and passing through a 140-mesh sieve to obtain a mixture;

[0064] (2) mixing the mixed material, the nanofiber colloid solution and the modified treatment liquid, ultrasonicating, centrifuging, filtering, washing with deionized water and drying to obtain a solid material;

[0065] (3) The solid material and the antioxidant are mixed and melted in a twin-screw extruder, extruded after stirring, and cooled to obtain a degradable, highly flexible, hydrophobic packaging material.

[0066] The mass ratio of polylactic acid, modified filler and deionized water in step (1) of this embodiment is 6.28:1.47:9; the molecular weight of the polylactic acid of this embodiment is 150000; the parameters of the ball milling step of this embodiment are: ball milling speed is 200rmp, and ball milling time is 25min.

[0067] The preparation method of the modified filler of this embodiment is:

[0068] The filler was crushed into 150 mesh, soaked in a 2 mol / L hydrochloric acid solution for 3 hours, filtered, and the obtained solid A was washed with deionized water, and then dried in an oven at 90°C for 4 hours to obtain a dry product; the dry product, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and anhydrous ethanol were added to a reactor, stirred and mixed, and then filtered. The obtained solid B was washed with anhydrous ethanol and then dried in an oven at 60°C for 7 hours to obtain a modified filler.

[0069] The filler of this embodiment is composed of clay mineral and talc in a mass ratio of 7.45:1.25; the clay mineral of this embodiment is kaolin; the mass ratio of the dried product, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and anhydrous ethanol in this embodiment is 6.9:0.9:24; the filtration in this embodiment uses a 250-mesh filter cloth; the parameters of the reactor in this embodiment are: temperature of 65°C, rotation speed of 400rmp, and time of 3.5h.

[0070] The mass of the nanofiber colloidal solution in step (2) of this embodiment accounts for 11wt% of the mixture, and the mass of the modified treatment liquid of this embodiment accounts for 6.5wt% of the mixture; the parameters of the ultrasonic treatment of this embodiment are: ultrasonic frequency is 40kHz, ultrasonic power is 200W, ultrasonic temperature is 50℃, and ultrasonic time is 50min; the parameters of the centrifugal treatment of this embodiment are: centrifugal speed is 4000rmp, and centrifugal time is 15min.

[0071] The preparation method of the nanofiber colloid solution of this embodiment is:

[0072] Chlorella powder with a particle size of 150 mesh was added to deionized water and stirred at a speed of 450 rpm for 1.5 hours to obtain a suspension with a mass concentration of 2 wt%. The suspension was subjected to high-pressure homogenization, centrifugation, and the supernatant was collected and dialyzed to obtain a nanofiber colloidal solution.

[0073] The parameters of the high-pressure homogenization treatment in this embodiment are: homogenization pressure of 90 MPa, number of homogenizations of 4 times, homogenization time of 5 min, and each homogenization interval of 2 min; the parameters of the centrifugal treatment in this embodiment are: centrifugal speed of 8000 rpm, and centrifugal time of 15 min; the steps of the dialysis treatment in this embodiment are: pouring the supernatant into a dialysis bag with a molecular weight cutoff of 5000D, placing the dialysis bag in a container containing 2L of deionized water, replacing the deionized water every 4 hours, and the dialysis cycle is 24 hours.

[0074] The preparation method of the modified treatment liquid of this embodiment is:

[0075] Perfluorooctyltriethoxysilane, surfactant, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, potassium persulfate and ethanol solution were mixed in a mass ratio of 1.6:0.61:0.3:0.09:10.5, and stirred at a speed of 700 rpm for 2.5 hours to obtain a modified treatment solution.

[0076] The surfactant of this embodiment is sodium dodecylbenzene sulfonate; the mass concentration of the ethanol solution of this embodiment is 75wt%.

[0077] The mass of the antioxidant in step (3) of this embodiment accounts for 0.3wt% of the solid material, and the antioxidant in this embodiment is antioxidant 1010; the temperature of the melting step in step (3) of this embodiment is 165°C; the stirring speed in step (3) of this embodiment is 300rmp.

[0078] Comparative Example 1

[0079] On the basis of Example 3, the talc in the filler was removed and replaced with kaolin of equal weight, and other conditions were consistent with Example 3.

[0080] Comparative Example 2

[0081] On the basis of Example 3, the filler is not modified, and other conditions are consistent with Example 3.

[0082] Comparative Example 3

[0083] On the basis of Example 3, the nanofiber colloid solution was removed and replaced with an equal weight of the modified treatment solution. Other conditions were the same as those in Example 3.

[0084] Comparative Example 4

[0085] On the basis of Example 3, the perfluorooctyltriethoxysilane in the modified treatment solution was removed and replaced with an equal weight of γ-(2,3-epoxypropoxy)propyltrimethoxysilane. Other conditions were consistent with those in Example 3.

[0086] Comparative Example 5

[0087] On the basis of Example 3, the γ-(2,3-epoxypropoxy)propyltrimethoxysilane in the modified treatment solution was removed and replaced with an equal weight of perfluorooctyltriethoxysilane. Other conditions were consistent with those in Example 3.

[0088] The packaging materials prepared in Examples 1-3 and Comparative Examples 1-5 were used as specimens with a specification of 80 mm×10 mm×4 mm. The bending strength test was performed in accordance with the standard GB / T 1449-2005. The tensile strength and elongation at break were performed in accordance with the standard GB / T 1447-2005. The water absorption test for 72 h was performed in accordance with the standard GB / T 1034-2008. The test results are shown in Table 1 below.

[0089] Table 1 Test results

[0090]

[0091]

[0092] As shown in Table 1, the degradable high-flexibility hydrophobic packaging materials prepared by Examples 1-3 are superior to the packaging materials prepared by Comparative Examples 1-5 in terms of flexural strength, tensile strength and tensile elongation at break, and have a low 72h water absorption rate, and have good hydrophobic properties. This shows that the present invention effectively improves the compatibility between the materials and the flexibility of the substrate by blending polylactic acid, modified fillers and nanofiber colloid solutions, and then improves the hydrophobic properties from the inside of the molecule to the surface through the modified treatment liquid, thereby synergistically improving the flexibility and hydrophobic properties of the material.

[0093] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a degradable, highly flexible, hydrophobic packaging material, characterized in that: The preparation method comprises the following steps: (1) mixing polylactic acid, modified filler and deionized water, ball milling and passing through a 80-200 mesh sieve to obtain a mixture; (2) mixing the mixed material, the nanofiber colloid solution and the modified treatment liquid, ultrasonicating, centrifuging, filtering, washing with deionized water and drying to obtain a solid material; (3) The solid material and the antioxidant are mixed and melted in a twin-screw extruder, extruded after stirring, and cooled to obtain a degradable, highly flexible, hydrophobic packaging material.

2. The method for preparing a degradable high-flexibility hydrophobic packaging material according to claim 1, characterized in that: The mass ratio of the polylactic acid, the modified filler and the deionized water in the step (1) is 5.26-7.3:1.14-1.8:8-10; the molecular weight of the polylactic acid is 120000-180000; the parameters of the ball milling step are: the ball milling speed is 100-300rmp, and the ball milling time is 20-30min.

3. The method for preparing a degradable high-flexibility hydrophobic packaging material according to claim 2, characterized in that: The preparation method of the modified filler is: The filler is crushed into 100-200 mesh, soaked in 1-3 mol / L hydrochloric acid solution for 2-4 hours, filtered, and the obtained solid A is washed with deionized water, and then dried in a 90°C oven for 3-5 hours to obtain a dry product; the dry product, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and anhydrous ethanol are added to a reactor, stirred and mixed, and then filtered. The obtained solid B is washed with anhydrous ethanol and then dried in a 60°C oven for 6-8 hours to obtain a modified filler.

4. The method for preparing a degradable high-flexibility hydrophobic packaging material according to claim 3, characterized in that: The filler is composed of clay mineral and talc powder in a mass ratio of 6.8-8.1:0.8-1.7; the clay mineral is selected from one or more of montmorillonite, kaolin and illite; the mass ratio of the dried product, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and anhydrous ethanol is 5.2-8.6:0.7-1.1:18-30; the filtration uses a 200-300 mesh filter cloth; the parameters of the reactor are: temperature of 60-70°C, rotation speed of 300-500rmp, and time of 2.5-4.5h.

5. The method for preparing a degradable high-flexibility hydrophobic packaging material according to claim 1, characterized in that: The mass of the nanofiber colloidal solution in step (2) accounts for 10-12wt% of the mixture, and the mass of the modified treatment liquid accounts for 5-8wt% of the mixture; the parameters of the ultrasonic treatment are: ultrasonic frequency is 20-60kHz, ultrasonic power is 100-300W, ultrasonic temperature is 40-60℃, and ultrasonic time is 40-60min; the parameters of the centrifugal treatment are: centrifugal speed is 3000-5000rmp, and centrifugal time is 10-20min.

6. The method for preparing a degradable high-flexibility hydrophobic packaging material according to claim 5, characterized in that: The preparation method of the nanofiber colloid solution is: Chlorella powder with a particle size of 100-200 mesh is added to deionized water, and stirred at a speed of 400-500 rpm for 1-2 hours to obtain a suspension with a mass concentration of 1-3 wt%. The suspension is subjected to high-pressure homogenization, centrifugation, and the supernatant is collected and dialyzed to obtain a nanofiber colloidal solution.

7. The method for preparing a degradable high-flexibility hydrophobic packaging material according to claim 6, characterized in that: The parameters of the high-pressure homogenization treatment are: homogenization pressure of 80-100MPa, number of homogenizations of 4 times, homogenization time of 5min, and an interval of 2min between each homogenization; the parameters of the centrifugal treatment are: centrifugal speed of 6000-10000rmp, and centrifugal time of 10-20min; the steps of the dialysis treatment are: pouring the supernatant into a dialysis bag with a molecular weight cutoff of 4000-6000D, placing the dialysis bag in a container containing 2L of deionized water, replacing the deionized water every 4h, and the dialysis cycle is 24h.

8. The method for preparing a degradable high-flexibility hydrophobic packaging material according to claim 5, characterized in that: The preparation method of the modified treatment liquid is: Perfluorooctyltriethoxysilane, surfactant, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, potassium persulfate and ethanol solution are mixed in a mass ratio of 1.4-1.8:0.52-0.7:0.25-0.35:0.07-0.11:9-12, and stirred at a speed of 600-800 rpm for 2-3 hours to obtain a modified treatment solution.

9. The method for preparing a degradable high-flexibility hydrophobic packaging material according to claim 8, characterized in that: The surfactant is selected from one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and Tween-80; the mass concentration of the ethanol solution is 70-80wt%.

10. The method for preparing a degradable high-flexibility hydrophobic packaging material according to claim 1, characterized in that: The mass of the antioxidant in step (3) accounts for 0.1-0.5wt% of the solid material, and the antioxidant is selected from one or more of antioxidant 1010 and antioxidant 168; the temperature of the melting step in step (3) is 150-180°C; the stirring speed in step (3) is 100-500rmp.