Modified epoxy resin anticorrosive coating material as well as preparation method and application thereof
By introducing bisphenol A-type polyarylether nitrile into epoxy resin to form a semi-interpenetrating network structure, the toughness and corrosion resistance issues of epoxy resin coatings are solved, and their service life in marine environments is improved.
Patent Information
- Application Number
- CN202411000322.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
Existing epoxy resin coatings have poor impact resistance and are prone to cracking after curing. Furthermore, volume shrinkage during the curing process leads to microporous defects, which affects their corrosion resistance in marine environments.
Epoxy resin was modified with bisphenol A type polyarylether nitrile and uniformly dispersed in the epoxy resin matrix by solution blending to form a semi-interpenetrating network structure, which filled micropores and improved toughness and mechanical properties.
It significantly improves the toughness and mechanical properties of epoxy resin, reduces shrinkage, and enhances corrosion resistance, making it suitable for protection in harsh environments such as offshore wind turbine towers.
Smart Images

Figure CN118931309A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite protective materials, and specifically relates to a modified epoxy resin anticorrosive coating material and a preparation method and application thereof. Background Art
[0002] In recent years, my country has attached increasing importance to the development of the marine economy, and the construction of the marine economy has greatly driven the demand for anti-corrosion coatings. However, so far, traditional materials are facing severe corrosion problems in the face of application needs in the marine environment. Although the design life of many major marine projects is usually 50 years or even hundreds of years, the service life of the project is far from expected in the harsh marine corrosion environment. Offshore wind power towers face harsh marine climates, not only because they are in high salt fog, high humidity, high-intensity ultraviolet rays and large day and night temperature differences for a long time, but also because the surface of the tower is rusted and a thin film of accumulated water is formed under the continuous scouring of seawater. The high salt content of seawater has electrochemical reaction conditions, which further accelerates the corrosion rate of the tower steel structure equipment, seriously affecting the service life of the tower. Therefore, it is necessary to use suitable coating materials and coating processes to ensure the service life of the tower, extend its service life, and ensure the safe use of offshore wind power.
[0003] Epoxy resin coating has great application prospects in the petroleum, aerospace, construction and manufacturing industries due to its high adhesion to the substrate, excellent chemical and heat resistance, and high cost performance. However, epoxy resin has an extremely high cross-linking density after curing, which seriously damages the energy absorption capacity of epoxy resin under impact and stress. Therefore, the cured epoxy resin shows natural brittleness, poor impact resistance, and easy cracking. In addition, the epoxy resin coating will shrink in volume during the curing process, and when the solvent evaporates, it will inevitably produce micropore defects, making it easier for the corrosive medium to penetrate the coating and reach the surface of the substrate to cause corrosion reactions, which greatly limits the further development of epoxy resin in related fields.
[0004] At present, most of the protective materials for epoxy resin are introduced into epoxy resin by blending method, so as to improve the corrosion resistance, wear resistance, hydrophobicity and flexibility of epoxy resin coating. For example, in the prior art, a Chinese patent with publication number CN105440584A and application date of December 10, 2015 discloses a low shrinkage epoxy resin system and a preparation method thereof, wherein the low shrinkage epoxy resin system comprises the following components in parts by weight: 90-110 parts of bisphenol A epoxy resin, 15-25 parts of epoxy diluent, 40-60 parts of curing agent, 1-3 parts of coupling agent, and 4-7 parts of nano barium titanate powder. The low shrinkage epoxy resin obtained by the invention has a 50% lower shrinkage rate than the bulk resin, while the mechanical properties of the epoxy resin remain unchanged; the Chinese patent with publication number CN106280262A and application date of August 25, 2016 provides a fast-curing low linear shrinkage epoxy resin composition, the epoxy resin composition is composed of epoxy resin, amine curing agent and additives, the ratio of the epoxy equivalent of the epoxy resin to the active hydrogen equivalent of the amine curing agent is 1.0 / 0.8 to 1.0 / 1.2; the epoxy resin includes 1% cyclopentane The total weight of the epoxy resin is 85-100% of the aromatic epoxy resin and the total weight of the epoxy resin is 0-15% of the aliphatic epoxy resin and / or alicyclic epoxy resin; the aliphatic amine curing agent and / or alicyclic amine curing agent in the amine curing agent accounts for 60-100% of the total weight of the amine curing agent; the amount of additives added is 0-50% of the total weight of the epoxy resin and the amine curing agent, and the gel time of the epoxy resin composition at 120°C is less than 170 seconds, and the linear shrinkage after curing is less than 1.0%, achieving the effect of fast curing and low linear shrinkage. However, the above-mentioned prior art focuses on solving how to reduce the curing time of the epoxy resin and the shrinkage after curing, and cannot eliminate or alleviate the impact of the voids caused by the objective volume shrinkage after the epoxy resin is cured.
[0005] In view of this situation, in-depth research was conducted on special additive modified anti-corrosion coating materials and their preparation methods, and a modified epoxy resin anti-corrosion coating material with excellent chemical corrosion resistance was designed, so that not only the volume shrinkage rate is extremely low during the curing process, but also the gaps caused by volume shrinkage can be filled to improve the anti-corrosion performance. This can effectively solve the problem of poor comprehensive corrosion and wear resistance of existing anti-corrosion coatings available for offshore wind turbine towers, and has important practical value and research significance for the optimization of various equipment in marine engineering. Summary of the invention
[0006] In order to solve the problems existing in the prior art, the present invention provides a modified epoxy resin anti-corrosion coating material and a preparation method and application thereof. The modified epoxy resin anti-corrosion coating material overcomes the poor impact resistance and voids caused by volume shrinkage of the epoxy resin after curing, and has good mechanical properties, thermal properties and corrosion resistance.
[0007] The technical solution of the present invention is as follows:
[0008] One of the purposes of the present invention is to provide a method for preparing a modified epoxy resin anti-corrosion coating material, wherein bisphenol A type polyarylethernitrile is completely dissolved in cyclohexanone by heating and stirring, and then introduced into and uniformly dispersed in an epoxy resin coating matrix by solution blending to obtain the anti-corrosion coating material.
[0009] Further, the following steps are included:
[0010] S1, weighing bisphenol A type polyarylether nitrile and cyclohexanone by weight, and completely dissolving the bisphenol A type polyarylether nitrile in the cyclohexanone by heating and stirring;
[0011] S2, introducing the mixture of bisphenol A type polyarylether nitrile and cyclohexanone into the epoxy resin by solution blending, and uniformly dispersing the bisphenol A type polyarylether nitrile in the epoxy resin matrix by mechanical stirring;
[0012] S3, weighing a curing agent and a diluent, adding them to the bisphenol A type polyarylether nitrile / epoxy resin matrix mixed evenly in S2, and stirring evenly to obtain the modified epoxy resin anticorrosive coating material.
[0013] Furthermore, the raw materials of the modified epoxy resin anti-corrosion coating material are composed as follows:
[0014] Epoxy resin: 200-300 parts;
[0015] Bisphenol A type polyarylether nitrile: 4-30 parts;
[0016] Cyclohexanone: 32-240 parts;
[0017] Curing agent: 10-30 parts;
[0018] Diluent: 4-45 parts.
[0019] Furthermore, the heating condition in S1 is 25-35°C.
[0020] Furthermore, the stirring method in S1 is magnetic stirring.
[0021] Furthermore, the mechanical stirring method in S2 is an electric stirrer.
[0022] Furthermore, the curing agent in S3 is epoxy graphene zinc powder primer curing agent.
[0023] Furthermore, the diluent in S3 is an epoxy resin diluent.
[0024] A second object of the present invention is to provide a modified epoxy resin anti-corrosion coating material.
[0025] The third object of the present invention is to provide an application of a modified epoxy resin anti-corrosion coating material in the anti-corrosion coating of an offshore wind power tower.
[0026] Furthermore, the prepared modified epoxy resin anti-corrosion coating material was sprayed on the offshore wind power tower steel plate, the steel plate was cured at room temperature for 6 hours, and then placed in a 120° C. forced air oven for curing for 1 hour to obtain the anti-corrosion coating.
[0027] Compared with the prior art, the beneficial effects of the present invention are:
[0028] 1. The present invention adopts bisphenol A type polyarylether nitrile to modify epoxy resin for the first time to prepare an anti-corrosion coating material. Under the action of external force and deformation, the cyano group on the main chain of the bisphenol A type polyarylether nitrile in the anti-corrosion coating material forms hydrogen bonds with the hydroxyl group after the epoxy resin is opened, and a semi-interpenetrating network structure is constructed in the epoxy resin system, providing additional energy dissipation paths and stress damping sites, thereby playing a bridging constraint role and inducing the closure of epoxy resin cracks, preventing the expansion of epoxy resin cracks, and significantly improving the toughness and comprehensive mechanical properties of the epoxy resin.
[0029] 2. The macromolecules of bisphenol A type polyarylether nitrile are difficult to form a straight and stretched linear configuration due to the main chain, which destroys their tight stacking and makes it difficult to form crystals. The gaps between the main chains of the polymer can be increased, which is beneficial to the penetration of small molecules of organic solvents. In addition, the macromolecules of bisphenol A type polyarylether nitrile have excellent chemical corrosion resistance and extremely low shrinkage performance. Therefore, the anti-corrosion coating material modified by bisphenol A type polyarylether nitrile in the present invention can not only reduce the shrinkage rate during the curing process of epoxy resin and avoid the generation of residual stress during the curing process, but also fill the microporous structure generated after curing that can be penetrated by corrosive media, thereby further improving the anti-corrosion performance of the coating material.
[0030] 3. The present invention utilizes a large number of methyl groups (-CH3) on the main chain of bisphenol A type polyarylether nitrile to reduce the rigidity of the polymer molecular chain, and promotes the free movement of the molecular chain segments through its good solubility and processing fluidity, so that bisphenol A type polyarylether nitrile exhibits good compatibility when blended with epoxy resin or dissolved in non-polar solvents such as cyclohexanone, thereby simplifying the preparation process of the anti-corrosion coating material and the application steps and difficulty on metal workpieces, which is conducive to industrial production and the expansion of other application fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a SEM image of the modified epoxy resin anti-corrosion coating material described in Example 1 of the present invention;
[0032] Figure 2 It is a DSC curve diagram of the modified epoxy resin anticorrosive coating material described in the performance test of the present invention;
[0033] Figure 3 It is the Niquist diagram of the modified epoxy resin anti-corrosion coating material described in the performance test of the present invention. DETAILED DESCRIPTION
[0034] The present invention is further described below in conjunction with preferred embodiments. The endpoints of the ranges disclosed in the present invention and any values are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be deemed to be specifically disclosed herein.
[0035] The experimental methods in the following examples, unless otherwise specified, are conventional methods and are performed according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0036] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0037] Example 1
[0038] This embodiment provides a modified epoxy resin anti-corrosion coating material, and the preparation method thereof comprises the following steps:
[0039] S1. Weigh 4 g of bisphenol A poly(arylene ether nitrile) and 32 g of cyclohexanone, and heat and magnetically stir at 30° C. to completely dissolve the bisphenol A poly(arylene ether nitrile) in the cyclohexanone.
[0040] S2, using solution blending to introduce the bisphenol A type polyarylether nitrile and cyclohexanone mixture into 200g of epoxy micaceous iron resin, and using an electric stirrer to mechanically stir so that the bisphenol A type polyarylether nitrile is uniformly dispersed in the epoxy micaceous iron resin matrix;
[0041] S3, weigh 10g of epoxy graphene zinc powder primer curing agent and 4g of epoxy resin diluent, add the bisphenol A type polyarylether nitrile / epoxy micaceous iron resin matrix mixed evenly in S2, and stir evenly to obtain the modified epoxy micaceous iron resin anti-corrosion coating material Z2.
[0042] Example 2
[0043] This embodiment provides a modified epoxy resin anti-corrosion coating material, and the preparation method thereof comprises the following steps:
[0044] S1, weighing 8 g of bisphenol A type polyarylether nitrile and 64 g of cyclohexanone, heating and magnetic stirring at 25° C. to completely dissolve the bisphenol A type polyarylether nitrile in the cyclohexanone;
[0045] S2, introducing the mixture of bisphenol A type polyarylether nitrile and cyclohexanone into 220g of epoxy micaceous iron resin by solution blending, and uniformly dispersing the bisphenol A type polyarylether nitrile in the epoxy micaceous iron resin matrix by mechanical stirring with an electric stirrer;
[0046] S3, weigh 15g of epoxy graphene zinc powder primer curing agent and 15g of epoxy resin diluent, add the bisphenol A type polyarylether nitrile / epoxy micaceous iron resin matrix mixed evenly in S2, and stir evenly to obtain the modified epoxy micaceous iron resin anti-corrosion coating material Z4.
[0047] Example 3
[0048] This embodiment provides a modified epoxy resin anti-corrosion coating material, and the preparation method thereof comprises the following steps:
[0049] S1. Weigh 16 g of bisphenol A poly(arylene ether nitrile) and 96 g of cyclohexanone, and heat and magnetically stir at 35° C. to completely dissolve the bisphenol A poly(arylene ether nitrile) in the cyclohexanone.
[0050] S2, introducing the mixture of bisphenol A type polyarylether nitrile and cyclohexanone into 250g of epoxy micaceous iron resin by solution blending, and uniformly dispersing the bisphenol A type polyarylether nitrile in the epoxy micaceous iron resin matrix by mechanical stirring with an electric stirrer;
[0051] S3, weigh 20g of epoxy graphene zinc powder primer curing agent and 25g of epoxy resin diluent, add them into the bisphenol A type polyarylether nitrile / epoxy micaceous iron resin matrix mixed evenly in S2, and stir evenly to obtain the modified epoxy micaceous iron resin anti-corrosion coating material Z6.
[0052] Example 4
[0053] This embodiment provides a method for preparing a modified epoxy resin anti-corrosion coating material, comprising the following steps:
[0054] S1, weighing 24g of bisphenol A type polyarylether nitrile and 160g of cyclohexanone, heating at 30°C and stirring with magnetic force to completely dissolve the bisphenol A type polyarylether nitrile in the cyclohexanone;
[0055] S2, introducing the mixture of bisphenol A type polyarylether nitrile and cyclohexanone into 270g of epoxy micaceous iron resin by solution blending, and uniformly dispersing the bisphenol A type polyarylether nitrile in the epoxy micaceous iron resin matrix by mechanical stirring with an electric stirrer;
[0056] S3, weigh 25g of epoxy graphene zinc powder primer curing agent and 35g of epoxy resin diluent, add the bisphenol A type polyarylether nitrile / epoxy micaceous iron resin matrix mixed evenly in S2, and stir evenly to obtain the modified epoxy micaceous iron resin anti-corrosion coating material Z8.
[0057] Example 5
[0058] This embodiment provides a method for preparing a modified epoxy resin anti-corrosion coating material, comprising the following steps:
[0059] S1, weighing 30g of bisphenol A type polyarylether nitrile and 240g of cyclohexanone, heating and magnetic stirring at 25°C to completely dissolve the bisphenol A type polyarylether nitrile in the cyclohexanone;
[0060] S2, using solution blending to introduce the bisphenol A type polyarylether nitrile and cyclohexanone mixture into 300g of epoxy micaceous iron resin, and using an electric stirrer to mechanically stir so that the bisphenol A type polyarylether nitrile is uniformly dispersed in the epoxy micaceous iron resin matrix;
[0061] S3, weigh 30g of epoxy graphene zinc powder primer curing agent and 45g of epoxy resin diluent, add the bisphenol A type polyarylether nitrile / epoxy micaceous iron resin matrix mixed evenly in S2, and stir evenly to obtain the modified epoxy micaceous iron resin anti-corrosion coating material Z10.
[0062] Comparative Example 1
[0063] This embodiment provides a method for preparing an epoxy resin anti-corrosion coating material, comprising the following steps:
[0064] S1, weigh 96g of cyclohexanone and introduce 250g of epoxy micaceous iron resin, and uniformly disperse the cyclohexanone in the epoxy micaceous iron resin matrix by mechanical stirring;
[0065] S3, weigh 20g of epoxy graphene zinc powder primer curing agent and 25g of epoxy resin diluent, add them into the epoxy micaceous iron resin matrix mixed evenly in S1, and stir evenly to obtain the epoxy micaceous iron resin anti-corrosion coating material Z0.
[0066] Performance Testing
[0067] The sample Z6 prepared in Example 3 was sprayed on a sandblasted steel plate (thickness 140-200 um). The sprayed steel plate was first placed at room temperature for a period of time to allow the epoxy micaceous iron resin to solidify and the solvent to evaporate. Then, it was placed in a blast oven for heat treatment (120°C for 1h) to remove the solvent. Finally, a modified epoxy micaceous iron anti-corrosion coating was obtained as a composite material sample for performance testing.
[0068] 1. Temperature resistance test
[0069] Differential Scanning Calorimetry (DSC): Weigh a certain amount of sample and place it in a crucible. Place the sample and reference in the sample chamber and reference chamber of the DSC instrument respectively. Set the appropriate heating or cooling rate and start the programmed temperature control so that the sample and reference are subjected to thermal analysis in the same heating or cooling environment.
[0070] Thermal Gravimetric Analysis (TGA): Place the sample in the sample tray of the thermogravimetric analyzer, set the experimental conditions, start the thermogravimetric analyzer, and begin heating the sample. Observe and record the mass change of the sample during the heating process.
[0071] like Figure 2 As shown, the Tg of Z6 increased from 85.0℃ (Z0) to 95.6℃, and T5% increased from 399℃ (Z0) to 405℃, indicating that the introduction of special additive bisphenol A type polyarylether nitrile into the epoxy zinc-rich primer coating can improve its thermal properties to a certain extent.
[0072] 2. Adhesion test
[0073] Use air blowing to make the surface of the sample smooth and clean, free of impurities and stains, then fix the sample on the tensile platform, ensure that the contact between the sample and the platform is firm and the surface of the sample is parallel to the platform; use a tensile machine to apply tensile force at a certain speed; during the load application process, record the tensile load applied to the sample; observe adhesion failure, and continue to apply tensile force until the adhesion between the sample and the substrate fails. The sign of adhesion failure can be the breakage of the sample or separation from the substrate.
[0074] Experiments show that Z6 has excellent adhesion (>14.2N / cm2), low water absorption (3.7%), low viscosity (554MPa / s) and high hardness (3H). The special additive bisphenol A type polyarylether nitrile helps to improve the adhesion between the primer and the metal. This can be attributed to the special group contained in the molecular side chain of the special additive bisphenol A type polyarylether nitrile, namely the cyano group. The cyano group has better adhesion to the metal, which can effectively improve the adhesion between the polymer and the metal, and ultimately lead to an increase in the adhesion between the primer and the iron sheet.
[0075] 3. Salt spray test
[0076] Prepare a 10% sodium chloride solution, install the test sample on the test fixture, and ensure good contact between the sample and the fixture. Set the salt spray test machine parameters, test temperature is 35℃, humidity is 95%, spray time is 24 hours, and interval time is 6-8 hours. Start the salt spray test machine and let the sodium chloride solution start spraying. Regularly check the appearance and performance of the test sample during the test and record the test data.
[0077] The 72h salt spray aging test proved that Z6 has excellent corrosion resistance and aging resistance, indicating that the single-layer primer coating after spraying has a good anti-corrosion effect.
[0078] 4. EIS test
[0079] The corrosion resistance of the modified epoxy micaceous iron intermediate coating was further studied by EIS test. Before immersion in 3.5wt% NaCl solution, the impedance of Z6 can reach 2.37×10 9 Ω.cm 2 , and when the electrode was immersed in 3.5wt% NaCl solution for 240h, the impedance of Z6 could still reach 9.29×10 8 Ω.cm 2 , indicating that with the increasing content of special additive bisphenol A polyarylethernitrile introduced into the epoxy primer, the modified primer coating has better corrosion resistance.
[0080] like Figure 3 As shown, the impedances of the Z0, Z2, Z4, Z6, Z8, and Z10 coatings are 2.17×10 7 , 2.36×10 9 , 2.87×10 9 , 9.29×10 9 , 1.25×10 9 and 3.24×10 9 Ω·cm 2 , and not at 3.5wt%
[0081] Compared with the intermediate paint coated electrode immersed in NaCl solution, the impedance values of all coatings decreased, but still had good corrosion resistance, especially the intermediate paint coating with the addition of special additive bisphenol A type polyarylethernitrile.
[0082] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a modified epoxy resin anticorrosive coating material, It is characterized in that The bisphenol A type polyarylethernitrile is completely dissolved in cyclohexanone by heating and stirring, and then introduced into and uniformly dispersed in the epoxy resin coating matrix by solution blending to obtain the anti-corrosion coating material.
2. A method for preparing a modified epoxy resin anticorrosive coating material according to claim 1, It is characterized in that The steps include: S1, weighing bisphenol A type polyarylether nitrile and cyclohexanone by weight, and completely dissolving the bisphenol A type polyarylether nitrile in the cyclohexanone by heating and stirring; S2, introducing the mixture of bisphenol A type polyarylether nitrile and cyclohexanone into the epoxy resin by solution blending, and uniformly dispersing the bisphenol A type polyarylether nitrile in the epoxy resin matrix by mechanical stirring; S3, weighing a curing agent and a diluent, adding them to the bisphenol A type polyarylether nitrile / epoxy resin matrix mixed evenly in S2, and stirring evenly to obtain the modified epoxy resin anticorrosive coating material.
3. A method for preparing a modified epoxy resin anticorrosive coating material according to claim 2, It is characterized in that The raw materials of the modified epoxy resin anticorrosive coating material are as follows: Epoxy resin: 200-300 parts; Bisphenol A type polyarylether nitrile: 4-30 parts; Cyclohexanone: 32-240 parts; Curing agent: 10-30 parts; Diluent: 4-45 parts.
4. A method for preparing a modified epoxy resin anticorrosive coating material according to claim 2, It is characterized in that The heating condition in S1 is 25-35°C.
5. A method for preparing a modified epoxy resin anticorrosive coating material according to claim 2, It is characterized in that The stirring method in S1 is magnetic stirring.
6. A method for preparing a modified epoxy resin anticorrosive coating material according to claim 2, It is characterized in that The mechanical stirring method in S2 is an electric stirrer.
7. A method for preparing a modified epoxy resin anticorrosive coating material according to claim 2, It is characterized in that The curing agent in S3 is epoxy graphene zinc powder primer curing agent.
8. A method for preparing a modified epoxy resin anticorrosive coating material according to claim 2, It is characterized in that The diluent in S3 is epoxy resin diluent.
9. A modified epoxy resin anticorrosive coating material prepared according to the method according to any one of claims 1 to 8.
10. Use of a modified epoxy resin anti-corrosion coating material prepared according to the method of any one of claims 1 to 8 in an offshore wind power tower anti-corrosion coating.
Citation Information
Patent Citations
Polyarylether nitrile / epoxy resin copolymerized modified composition and preparation method and application thereof
CN104045978A
Epoxy resin composition as well as preparation method and application thereof
CN113004654A
Phenolphthalein polyarylether sulfone modified montmorillonite toughened epoxy coating and preparation method thereof
CN114940854A
Resin composition and adhesive film and printed circuit board containing same
CN115819926A
Cited By
Preparation method of novel tough epoxy resin anticorrosive coating
CN120137499A