Rubber material for preparing temperature-resistant and oil-resistant automobile pipeline rubber product and preparation method thereof

By combining modified polyketone and glass powder with polyamide resin, the problem of easy hydrolysis of polyamide materials is solved, and its durability and mechanical properties in high temperature and oil environments are improved, and it is suitable for the manufacturing of automobile pipelines.

CN118931172APending Publication Date: 2024-11-12WENZHOU DEBANG POLYMER TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411254077.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing polyamide materials are easy to hydrolyze, resulting in a shortened service life in high temperature and oil environments, and it is difficult to meet the temperature and oil resistance requirements of automobile pipelines.

Method used

ABS resin is used to modify polyketone to prepare modified polyketone masterbatches, and glass powder is prepared with raw materials such as sodium oxide, calcium oxide, boron oxide, alumina and silicon oxide, and combined with modified polyketone masterbatches and poly Amide resin is prepared by melt blending of twin screw machines to improve its hydrolysis resistance and mechanical strength.

Benefits of technology

It significantly improves the hydrolysis resistance and mechanical strength of polyamide materials, extends service life, and maintains good performance in high temperature environments, and is suitable for the manufacturing of automobile pipelines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005033421580000081
    Figure BDA0005033421580000081
  • Figure BDA0005033421580000091
    Figure BDA0005033421580000091
Patent Text Reader

Abstract

The invention provides a rubber material for preparing a temperature-resistant and oil-resistant automobile pipeline rubber product and a preparation method of the rubber material. The preparation method comprises the following steps: S100, carrying out modification treatment on polyketone by adopting ABS (Acrylonitrile Butadiene Styrene) resin to prepare modified polyketone master batches; s200, preparing glass powder from raw materials including sodium oxide, calcium oxide, boric oxide, aluminum oxide and silicon oxide; and S300, preparing the rubber material from raw materials including the modified polyketone master batch, glass powder and polyamide resin. The rubber material provided by the invention is not easy to hydrolyze and has good processability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a rubber material for preparing heat-resistant and oil-resistant automobile pipeline rubber products and a preparation method thereof. Background Art

[0002] Automobile hose is one of the important components in the automobile system, which undertakes the task of conveying various liquids and gases. There are many types of automobile hoses, and each hose has its specific purpose and performance requirements. In the normal operation of the car, the reasonable use and maintenance of automobile hoses are essential to ensure the safety and reliability of the car. With the continuous development of automobile technology, automobile hoses are also constantly innovating and improving to meet the requirements of higher performance and safety. According to different uses and performance requirements, automobile hoses can be divided into many types. For example: coolant hoses are used to convey engine coolant, fuel hoses are used to convey fuel to the engine, and brake hoses are used to transmit brake fluid pressure. According to different braking forms, they are divided into hydraulic brake hoses, pneumatic brake hoses and vacuum brake hoses. In terms of materials, common automobile hoses are mainly rubber brake hoses and nylon brake hoses. Rubber hoses have strong tensile strength and are easy to install, while nylon hoses have the characteristics of light specific gravity, good flexibility and oil resistance.

[0003] Polyamide is a polymer containing amide groups in the repeating units of the macromolecular main chain. After being processed and modified, it can be widely used in automobile system pipelines such as fuel pipes, cooling pipes and brake oil pipes. However, one of the shortcomings of polyamide materials in the prior art is that polyamide materials are easily hydrolyzed. The hydrolysis of polyamide materials refers to the amide bonds (-CONH-) in the polyamide molecular chain being attacked by water molecules or other solvent molecules under specific conditions (such as the presence of acid, alkali or enzyme, and heating, etc.), resulting in the amide bond breaking, and then triggering the degradation and decomposition process of the polyamide molecular chain. Specifically, the hydrolysis process can reduce the molecular weight of polyamide and may form monomers, oligomers and other by-products. After hydrolysis, the tensile strength and elongation at break of the polyamide material will be significantly reduced, and its dimensional stability will be affected. Therefore, how to avoid the hydrolysis of polyamide materials and improve their service life is a technical problem that those skilled in the art need to solve. Summary of the invention

[0004] One of the problems solved by the present invention is how to provide a polyamide rubber material for the rubber core of an automobile hose which has a long service life and is not easy to hydrolyze.

[0005] In order to solve at least one of the above problems, the present invention provides a method for preparing a rubber material for preparing a heat-resistant and oil-resistant automobile pipeline rubber product, the preparation method comprising:

[0006] S100, modifying polyketone using ABS resin to prepare modified polyketone masterbatch;

[0007] S200, preparing glass powder using raw materials including sodium oxide, calcium oxide, boron oxide, aluminum oxide and silicon oxide;

[0008] S300, preparing a rubber material using raw materials including modified polyketone masterbatch, glass powder and polyamide resin.

[0009] In the above technical solution, S100 specifically includes:

[0010] S110, uniformly mixing an antioxidant, a lubricant, an ABS resin and a polyketone to obtain a first mixture;

[0011] S120, feeding the first mixture into a twin-screw extruder, melt blending, extruding and granulating, and preparing a modified polyketone masterbatch.

[0012] In the above technical solution, in S110, the mass ratio of antioxidant: lubricant: ABS resin: polyketone is (0.5-1): (4-6): (20-25): 100.

[0013] In the above technical solution, in S120, the temperature condition of melt blending is 210° C. to 240° C., the time of melt blending is 0.5 h to 1 h, and the speed condition of the twin-screw extruder is 200 r / min to 300 r / min.

[0014] In the above technical solution, the antioxidant is dilauryl thiodipropionate, and the lubricant is polytetrafluoroethylene.

[0015] In the above technical solution, S200 specifically includes:

[0016] S210, grinding and mixing sodium oxide, calcium oxide, boron oxide, aluminum oxide and silicon oxide to obtain a glass matrix;

[0017] S220, heating and melting the glass matrix to obtain glass liquid;

[0018] S230, quenching, cooling and grinding the glass liquid to obtain glass powder.

[0019] In the above technical scheme, in S210, in terms of mass ratio, sodium oxide:calcium oxide:boron oxide:aluminum oxide:silicon oxide = (2-5):(5-10):(5-30):(20-30):(40-55); and 0.17≤R2O / (SiO2+Al2O3)≤0.2, wherein R2O is the total mass of sodium oxide and calcium oxide, and SiO2+Al2O3 is the total mass of aluminum oxide and silicon oxide.

[0020] In the above technical solution, in S220, the temperature condition for heating and melting is 1100° C. to 1300° C., and the time for heating and melting is 2 h to 2.5 h.

[0021] In the above technical solution, S300 specifically includes:

[0022] S310, mixing oxidized polyethylene wax, tris(2,4-di-tert-butylphenyl)phosphite, diisononyl phthalate, maleic anhydride, glass powder, modified polyketone masterbatch and polyamide resin in a mass ratio of oxidized polyethylene wax: tris(2,4-di-tert-butylphenyl)phosphite: diisononyl phthalate: maleic anhydride: glass powder: modified polyketone masterbatch: polyamide resin = (0.5-1): (1-2): (2-4): (6-8): (10-20): (20-30): 100 to obtain a second mixture;

[0023] S320, feeding the second mixture into a twin-screw extruder, melt-blending for 1 h to 1.5 h at a temperature of 220° C. to 260° C. and a screw speed of 250 r / min to 300 r / min, extruding and granulating to obtain a rubber material.

[0024] The present invention also provides a rubber material for preparing heat-resistant and oil-resistant automobile pipeline rubber products. The rubber material is obtained by using the preparation method of any of the above technical solutions.

[0025] Beneficial Effects

[0026] The present invention provides a method for preparing a rubber material for preparing a heat-resistant and oil-resistant automobile pipeline rubber product. The method first uses ABS resin to modify polyketone to prepare a modified polyketone masterbatch. Then, raw materials including sodium oxide, calcium oxide, boron oxide, aluminum oxide and silicon oxide are used to prepare glass powder. Finally, raw materials including modified polyketone masterbatch, glass powder and polyamide resin are used to prepare a rubber material. Polyketone is a polymer material formed by coordination polymerization of carbon monoxide, ethylene and propylene, which has excellent hydrolysis resistance, excellent wear resistance, fuel resistance, impact resistance, high bending strength and gas barrier performance. In addition, polyketone also has a high heat deformation temperature and can be used for a long time under high temperature environmental conditions. Therefore, the present invention uses polyketone and polyamide resin to compound and jointly prepare a rubber material for preparing a heat-resistant and oil-resistant automobile pipeline rubber product. Polyketone can significantly improve the hydrolysis resistance of polyamide materials. Considering the presence of carbonyl carbon structure in polyketone resin, the aldol condensation reaction between molecules and within molecules during the melt processing is cross-linked, resulting in a rapid increase in viscosity of the polyketone resin during the melt process, easy adhesion in the equipment, resulting in difficulty in cleaning the equipment, and uneven discharging. The present invention uses ABS resin to modify the polyketone used. ABS resin is a terpolymer of acrylonitrile (A)-butadiene (B)-styrene (S). ABS resin can work normally in an environment of -25°C to 60°C and has good heat and cold resistance. After ABS resin is blended with polyketone, the melt processing temperature of polyketone can be reduced, thereby widening its processing window, and ABS resin can reduce the curing and cross-linking phenomenon of polyketone during the processing process, and improve the processing fluidity and formability of polyketone. Glass powder, as an inorganic filler, can improve the hydrophobicity, mechanical strength, chemical stability and oil resistance of polyamide rubber materials, and reduce the water absorption rate of polyamide to prevent its hydrolysis. In summary, the rubber material prepared by the present invention using raw materials including modified polyketone masterbatch, glass powder and polyamide resin has good mechanical strength, oil resistance and temperature resistance, is not easy to hydrolyze, has a longer service life, and is particularly suitable for the manufacture of automobile pipelines. DETAILED DESCRIPTION

[0027] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the following is a detailed description of the specific embodiments of the present invention.

[0028] Unless otherwise specified, the reagents and raw materials used in the present invention can be purchased through commercial channels. The experimental methods in the following examples without specifying specific conditions are selected according to conventional methods and conditions, or according to the product specifications.

[0029] An embodiment of the present invention provides a method for preparing a rubber material for preparing a heat-resistant and oil-resistant automobile pipeline rubber product, the preparation method comprising:

[0030] S100, modifying polyketone using ABS resin to prepare modified polyketone masterbatch;

[0031] S200, preparing glass powder using raw materials including sodium oxide, calcium oxide, boron oxide, aluminum oxide and silicon oxide;

[0032] S300, preparing a rubber material using raw materials including modified polyketone masterbatch, glass powder and polyamide resin.

[0033] The purpose of the present invention is to provide a polyamide rubber material which is not easily hydrolyzed. The means for achieving the above purpose of the present invention is to add polyketone with excellent hydrolysis resistance and glass powder as a filler which can prevent polyamide from absorbing water into the polyamide rubber material.

[0034] Considering that polyketone has high viscosity after heating and melting, it is easy to adhere to the equipment and difficult to discharge uniformly, the present invention uses ABS resin to modify polyketone. In the present invention, ABS resin (i.e., acrylonitrile-butadiene-styrene terpolymer) is specifically copolymerized by three monomers of acrylonitrile (A), butadiene (B), and styrene (S). The present invention has no special restrictions on the source of ABS resin, which can be a commercial product or prepared according to a conventional preparation method well known to those skilled in the art. The preferred ABS resin in the present invention is: the mass proportion of acrylonitrile structural units is 20% to 30%, the mass proportion of butadiene structural units is 20% to 30%, and the mass proportion of styrene structural units is 40% to 50%.

[0035] In order to achieve the modification of polyketone, S100 specifically includes:

[0036] S110, uniformly mixing an antioxidant, a lubricant, an ABS resin and a polyketone to obtain a first mixture;

[0037] S120, feeding the first mixture into a twin-screw extruder, melt blending, extruding and granulating, and preparing a modified polyketone masterbatch.

[0038] Preferably, in S110, the mass ratio of antioxidant: lubricant: ABS resin: polyketone is (0.5-1): (4-6): (20-25): 100.

[0039] Preferably, in S110, the weight ratio of antioxidant: lubricant: ABS resin: polyketone is 0.5:5:25:100.

[0040] Preferably, in S120, the temperature condition of melt blending is 210° C. to 240° C., the time of melt blending is 0.5 h to 1 h, and the speed condition of the twin-screw extruder is 200 r / min to 300 r / min.

[0041] Preferably, the antioxidant is dilauryl thiodipropionate, and the lubricant is polytetrafluoroethylene.

[0042] The reason for adopting the above steps is that after ABS resin and polyketone are blended, the melt processing temperature of polyketone can be reduced, thereby widening its processing window, and ABS resin can reduce the solidification and cross-linking phenomenon of polyketone during processing, thereby improving the processing fluidity and formability of polyketone. Therefore, the modified polyketone masterbatch obtained by modifying ABS resin can not only effectively prevent the hydrolysis of polyamide, but also ensure uniform mixing and discharging during the melt extrusion of polyamide rubber material, thereby improving the processability of polyamide rubber material.

[0043] The present invention uses glass powder as an inorganic filler for polyamide rubber material. In order to manufacture the glass powder, S200 specifically includes:

[0044] S210, grinding and mixing sodium oxide, calcium oxide, boron oxide, aluminum oxide and silicon oxide to obtain a glass matrix;

[0045] S220, heating and melting the glass matrix to obtain glass liquid;

[0046] S230, quenching, cooling and grinding the glass liquid to obtain glass powder.

[0047] Preferably, in S210, in terms of mass ratio, sodium oxide:calcium oxide:boron oxide:aluminum oxide:silicon oxide=(2-5):(5-10):(5-30):(20-30):(40-55); and 0.17≤R2O / (SiO2+Al2O3)≤0.2, wherein R2O is the total mass of sodium oxide and calcium oxide, and SiO2+Al2O3 is the total mass of aluminum oxide and silicon oxide. Preferably, R2O / (SiO2+Al2O3)=0.19.

[0048] Preferably, in S220, the temperature condition for heating and melting is 1100° C. to 1300° C., and the time for heating and melting is 2 h to 2.5 h.

[0049] The reason for adopting the above steps is that in the synthesis of polyketone, palladium catalysts such as [N,N] bidentate palladium, α-diimine palladium, diphosphine palladium complex, etc. are required. Therefore, when the polyketone masterbatch is mixed with the polyamide resin and sheared at high temperature, the residual palladium catalyst therein will hydrolyze the palladium acyl group, reduce the palladium compound, and produce electron acceptors, which will catalyze the intramolecular and intermolecular condensation reactions of the polyketone, resulting in changes in the molecular structure of the polyketone and the breaking of chemical bonds, thereby reducing the heat resistance of the polyketone, thereby affecting the service life of the rubber material composited with polyketone and polyamide in a high temperature environment.

[0050] To this end, the present invention provides a technical solution for mixing alkaline glass powder with polyketone masterbatch and polyamide resin. With the above-mentioned component ratio, alkaline glass can be prepared. By controlling R2O / (SiO2+Al2O3) to between 0.17 and 0.2, the alkalinity of the glass can be controlled by controlling the content of alkali metal or alkaline earth metal oxide. When the alkaline glass powder is mixed with polyketone, the palladium metal catalyst remaining in the polyketone component can be removed, the polyketone can be prevented from generating electron acceptors, and the molecular structure change and chemical bond breaking of the polyketone can be prevented, thereby effectively improving the high-temperature service life of the rubber material composited with polyketone and polyamide.

[0051] In order to prepare the rubber material of polyketone and polyamide composite, S300 specifically includes:

[0052] S310, mixing oxidized polyethylene wax, tris(2,4-di-tert-butylphenyl)phosphite, diisononyl phthalate, maleic anhydride, glass powder, modified polyketone masterbatch and polyamide resin in a mass ratio of oxidized polyethylene wax: tris(2,4-di-tert-butylphenyl)phosphite: diisononyl phthalate: maleic anhydride: glass powder: modified polyketone masterbatch: polyamide resin = (0.5-1): (1-2): (2-4): (6-8): (10-20): (20-30): 100 to obtain a second mixture;

[0053] S320, feeding the second mixture into a twin-screw extruder, melt-blending for 1 h to 1.5 h at a temperature of 220° C. to 260° C. and a screw speed of 250 r / min to 300 r / min, extruding and granulating to obtain a rubber material.

[0054] The invention comprises the following steps: the oxidized polyethylene wax is used as a lubricant, the tris(2,4-di-tert-butylphenyl)phosphite is used as an antioxidant, the diisononyl phthalate is used as a plasticizer, and the maleic anhydride is used as a compatibilizer.

[0055] In the above steps, polyketone and polyamide resin are compounded to prepare a rubber material for preparing heat-resistant and oil-resistant automobile pipeline rubber products. Polyketone can significantly improve the hydrolysis resistance of polyamide materials, and ABS resin can improve the processing performance of polyketone, avoiding its adhesion in equipment, which makes it difficult to clean the equipment. Glass powder can improve the mechanical properties and mechanical strength of polyamide materials. In addition, alkaline glass can prevent the generation of electron acceptors in polyketone, thereby improving the high-temperature service life of rubber materials.

[0056] Example 1

[0057] This embodiment provides a rubber material for a rubber core of an automobile hose, which is prepared by the following steps:

[0058] S1. Mixing dilauryl thiopropionate, polytetrafluoroethylene, ABS resin and polyketone in a mass ratio of dilauryl thiopropionate: polytetrafluoroethylene: ABS resin: polyketone = 0.5:5:25:100 to obtain a first mixture;

[0059] S2. Feed the first mixture into a twin-screw extruder, melt blend for 1 hour, extrude and granulate to prepare a modified polyketone masterbatch; the twin-screw extruder has multiple heating zones from 1# to 10#, and the temperatures of the multiple heating zones and the die are set to 210°C, 210°C, 220°C, 220°C, 220°C, 235°C, 235°C, 230°C, 230°C, 240°C, 240°C in sequence; the screw speed of the main machine is 250r / min;

[0060] S3. Grind and mix sodium oxide, calcium oxide, boron oxide, aluminum oxide and silicon oxide according to the mass ratio in Table 1 to obtain a glass matrix, send the glass matrix into a resistance furnace, heat it to 1250° C. under nitrogen protection, heat it at 1250° C. for 2 hours to melt it, obtain glass liquid, pour the glass liquid into cold water for water quenching, quench it and grind it after cooling to obtain glass powder;

[0061] S4, mixing oxidized polyethylene wax, tris(2,4-di-tert-butylphenyl)phosphite, diisononyl phthalate, maleic anhydride, glass powder, modified polyketone masterbatch and PA6 polyamide resin in a mass ratio of oxidized polyethylene wax: tris(2,4-di-tert-butylphenyl)phosphite: diisononyl phthalate: maleic anhydride: glass powder: modified polyketone masterbatch: PA6 polyamide resin = 1:1:2:6:15:25:100 to obtain a second mixture;

[0062] S5. Feed the second mixture into a twin-screw extruder, melt blend for 1.5 hours, extrude and granulate to obtain a rubber material; the twin-screw extruder has multiple heating zones from 1# to 10#, and the temperatures of the multiple heating zones and the die are set to 220°C, 220°C, 230°C, 230°C, 240°C, 240°C, 245°C, 250°C, 250°C, 260°C, and 260°C in sequence; the screw speed of the main engine is 250r / min.

[0063] Table 1

[0064]

[0065]

[0066] Performance Testing

[0067] The performance test results of samples 1 to 9 are listed in Table 2. The accelerated aging test conditions for the above samples are ethanol hydrolysis aging at a temperature of 160°C for 1000 hours.

[0068] Table 2

[0069] Serial number Tensile strength(MPa) Tensile strength after aging test (MPa) Sample 1 52.8 35.5 Sample 2 51.5 36.3 Sample 3 49.3 37.4 Sample 4 51.7 37.8 Sample 5 50.8 44.2 Sample 6 49.1 43.7 Sample 7 51.4 45.8 Sample 8 50.1 39.1 Sample 9 48.8 38.5

[0070] It can be seen from the above test results that the tensile strength of samples 1 to 9 all reached more than 48MPa, which shows that the addition of glass powder helps to improve the mechanical strength of polyamide resin materials. Among them, samples 1 and sample 4 show higher mechanical properties. The applicant believes that this is due to the high content of silicon oxide and aluminum oxide added in the above two samples. After the high-temperature accelerated aging test, the tensile strength of samples 1 to sample 4, as well as samples 8 and sample 9 decreased significantly. The applicant believes that this is because the appropriate addition of alkali metal or alkaline earth metal oxides gives the glass powder a certain alkalinity, and the alkaline glass prevents the chemical bond breakage of polyketone, thereby effectively improving the high-temperature stability and service life of the rubber material composited with polyketone and polyamide. However, too high an alkali metal or alkaline earth metal oxide content will cause the silicon oxygen bond of the silicon oxygen tetrahedron in the glass to break, making the glass structure loose, increasing the thermal expansion coefficient of the glass, reducing the thermal stability and mechanical strength of the glass, especially reducing the thermal shock resistance of the glass, causing it to accumulate internal stress under long-term heating conditions, affecting the mechanical strength of the material.

[0071] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for preparing a rubber material for preparing a heat-resistant and oil-resistant automobile pipeline rubber product, characterized in that: The preparation method comprises: S100, modifying polyketone using ABS resin to prepare modified polyketone masterbatch; S200, preparing glass powder using raw materials including sodium oxide, calcium oxide, boron oxide, aluminum oxide and silicon oxide; S300, preparing the rubber material using raw materials including the modified polyketone masterbatch, the glass powder and polyamide resin.

2. The preparation method according to claim 1, characterized in that: S100 specifically includes: S110, uniformly mixing an antioxidant, a lubricant, the ABS resin and the polyketone to obtain a first mixture; S120, feeding the first mixture into a twin-screw extruder, melt blending, extruding and granulating, to prepare the modified polyketone masterbatch.

3. The preparation method according to claim 2, characterized in that: In S110, the mass ratio of antioxidant: lubricant: ABS resin: polyketone is (0.5-1): (4-6): (20-25):

100.

4. The preparation method according to claim 2, characterized in that: In S120, the temperature condition of the melt blending is 210° C. to 240° C., the time of the melt blending is 0.5 h to 1 h, and the speed condition of the twin-screw extruder is 200 r / min to 300 r / min.

5. The preparation method according to claim 2, characterized in that: The antioxidant is dilauryl thiodipropionate, and the lubricant is polytetrafluoroethylene.

6. The preparation method according to any one of claims 1 to 5, characterized in that S200 specifically includes: S210, grinding and mixing the sodium oxide, the calcium oxide, the boron oxide, the aluminum oxide and the silicon oxide to obtain a glass matrix; S220, heating and melting the glass matrix to obtain glass liquid; S230, quenching, cooling, and grinding the glass liquid to obtain the glass powder.

7. The preparation method according to claim 6, characterized in that: In S210, in terms of mass ratio, sodium oxide:calcium oxide:boron oxide:aluminum oxide:silicon oxide=(2-5):(5-10):(5-30):(20-30):(40-55); and 0.17≤R2O / (SiO2+Al2O3)≤0.2, wherein R2O is the total mass of the sodium oxide and the calcium oxide, and SiO2+Al2O3 is the total mass of the aluminum oxide and the silicon oxide.

8. The preparation method according to claim 6, characterized in that: In S220, the temperature condition of the heating and melting is 1100°C to 1300°C, and the time of the heating and melting is 2h to 2.5h.

9. The preparation method according to any one of claims 1 to 5, characterized in that S300 specifically includes: S310, uniformly mixing the oxidized polyethylene wax, the tris(2,4-di-tert-butylphenyl)phosphite, the diisononyl phthalate, the maleic anhydride, the glass powder, the modified polyketone masterbatch and the polyamide resin in a mass ratio of oxidized polyethylene wax: tris(2,4-di-tert-butylphenyl)phosphite: diisononyl phthalate: maleic anhydride: glass powder: modified polyketone masterbatch: polyamide resin = (0.5-1): (1-2): (2-4): (6-8): (10-20): (20-30): 100 to obtain a second mixture; S320, feeding the second mixture into a twin-screw extruder, melt-blending for 1 h to 1.5 h at a temperature of 220° C. to 260° C. and a screw speed of 250 r / min to 300 r / min, extruding and granulating to obtain the rubber material.

10. A rubber material for preparing heat-resistant and oil-resistant automobile pipeline rubber products, characterized in that: The rubber material is obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Automobile nylon tube and preparation method thereof