Method for producing thermally conductive polysiloxane composition

By designing silicone compounds as surface treatment agents, the problems of rising viscosity and uneven dispersion of thermally conductive silicone rubber during high filling are solved, and the thermal conductivity and operability are improved, and it is suitable for high-performance heat dissipation components.

CN118931196APending Publication Date: 2024-11-12MOMENTIVE PERFORMANCE MATERIALS JAPAN LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411128772.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2016-07-22
Filing Date
2017-07-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing thermally conductive silicone rubber increases viscosity and decreases fluidity when it is highly filled with inorganic particles, resulting in difficulty in operation, and uneven dispersion of fillers affects productivity. The heat resistance of the surface treatment agent is insufficient, making it difficult to meet high thermal conductivity and good quality. Processing requirements.

Method used

A silicone compound was designed as a surface treatment agent to improve the treatment efficiency and heat resistance of the thermally conductive filler through molecular structure optimization. The silicone compound with a cyclic structure and hydrolyzable group was used to phase silicone polymer. Combined, control the interaction of fillers with polymers, reduce viscosity and improve stability.

Benefits of technology

The excellent composition with thermal conductivity and operability is achieved, the filling rate and dispersion uniformity of the thermal conductivity filler are improved, the viscosity is reduced, the heat resistance and stability of the composition are enhanced, and it is suitable for high-performance heat dissipation members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004997232610000031
    Figure BDA0004997232610000031
  • Figure BDA0004997232610000032
    Figure BDA0004997232610000032
  • Figure BDA0004997232610000041
    Figure BDA0004997232610000041
Patent Text Reader

Abstract

The present application provides a method for producing a thermally conductive polysiloxane composition. Provided is a cyclic siloxane which is represented by general formula (1) (in the formula, R1, R2, R3, X, a, b, c, R4, Y and d are as defined in the description) and which has a hydrolyzable functional group containing an alkoxysilyl group and a linear polysiloxane structure having a specific length. This compound can be used as a surface treatment agent for a thermally conductive filler, said surface treatment agent being capable of providing a composition having excellent workability, thermal conductivity, and workability.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of a patent application with an application date of July 20, 2017, application number 201780038863.X, and invention name “Surface treatment agent for thermally conductive polyorganosiloxane composition”. Technical Field

[0002] The present invention relates to a siloxane compound for a surface treatment agent used in a thermally conductive polyorganosiloxane composition. Background Art

[0003] In electronic components such as power transistors, ICs, and CPUs, highly conductive thermal grease and thermally conductive sheets are used to prevent heat accumulation in the heat sink. Thermally conductive grease has the advantage of being easily applied regardless of the shape of the electronic component, but it has the problem of contaminating other components and oil leakage. In addition, although thermally conductive sheets do not contaminate other components or leak oil, their adhesion is worse than that of grease, so a method of reducing the hardness of the thermally conductive sheet is used to improve adhesion.

[0004] Thermally conductive sheets are mostly made of silicone rubber. However, since silicone alone cannot improve thermal conductivity, a thermally conductive filler is used in combination with silicone rubber to improve thermal conductivity. The following technology is known: adding a material with higher thermal conductivity than silicone as a binder, such as silica powder, alumina, boron nitride, aluminum nitride, and magnesium oxide, as a thermally conductive filler (Japanese Patent Publication No. 2002-003831).

[0005] However, when the filler containing the above-mentioned inorganic particles is directly filled into the silicone that becomes the binder, the viscosity of the composite material increases significantly in any case, resulting in a decrease in fluidity, which sometimes causes obstacles to operation. In addition, the filler used requires a considerable amount of time to achieve uniform dispersion, and productivity decreases. In order to solve these problems, it is proposed to perform surface treatment on the thermal conductive filler with various surface treatment agents to improve the filling property (please refer to Japanese Patent Publication No. 2000-1616, Japanese Patent Publication No. 2000-256558 and Japanese Patent Publication No. 2003-213133).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2002-003831

[0009] Patent Document 2: Japanese Patent Application Publication No. 2000-1616

[0010] Patent Document 3: Japanese Patent Application Publication No. 2000-256558

[0011] Patent Document 4: Japanese Patent Application Publication No. 2003-213133 Summary of the invention

[0012] Problem that the invention aims to solve

[0013] In order to achieve high heat dissipation as a heat dissipation component, inorganic particles such as alumina with a micro-particle size are surface-treated with hydrolyzable siloxane before use. However, along with high output, the heat dissipation of electronic components has also increased recently, and heat dissipation components with higher thermal conductivity are gradually required. In order to obtain a silicone composition with high thermal conductivity to meet the above needs, it is necessary to further highly fill the thermally conductive filler. Furthermore, it is also hoped that the obtained silicone composition has good handleability. On the other hand, the surface treatment agent used in the silicone rubber is not only required to be able to efficiently handle the thermally conductive filler, but also requires the surface treatment agent itself to have high heat resistance. Therefore, it is necessary to explore a surface treatment agent that provides a composition with excellent thermal conductivity and operability.

[0014] The present invention has been made to solve such a problem, and an object of the present invention is to provide a surface treatment agent for a thermally conductive filler that can provide a composition having excellent workability, thermal conductivity, and handling properties.

[0015] Means used to solve problems

[0016] In order to solve the above technical problems, the present inventors conducted intensive research and found that high filling can be achieved by designing the molecular structure of the surface treatment agent, thereby improving the thermal conductivity of the thermally conductive polysiloxane composition, thereby completing the present invention.

[0017] The present invention relates to the following items.

[0018] [1] A siloxane compound represented by the following general formula (1),

[0019] [Chemistry 1]

[0020]

[0021] (Where,

[0022] R 1 : A group having an alkoxysilyl group having 1 to 4 carbon atoms

[0023] R 2 : A linear organic siloxy group represented by the following general formula (2)

[0024] [Chemistry 2]

[0025]

[0026] (Where R4 are each independently a monovalent hydrocarbon group having 1 to 12 carbon atoms, Y is a monovalent hydrocarbon group having 1 to 6 carbon atoms, and d is an integer of 10 to 50)

[0027] X: Each independently represents a divalent hydrocarbon group having 2 to 10 carbon atoms

[0028] a and b: each independently an integer greater than 1

[0029] c: integer greater than 0

[0030] a+b+c: integer greater than 4

[0031] R 3 : each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms).

[0032] [2] The siloxane compound according to [1] above, wherein in the general formula (1), b is 2 and d is 10 to 40.

[0033] [3] The siloxane compound according to [1] above, wherein in the general formula (1), b is 1.

[0034] [4] A surface treatment agent for a thermally conductive filler, comprising the siloxane compound according to any one of [1] to [3] above.

[0035] Effects of the Invention

[0036] According to the present invention, it is possible to provide a surface treatment agent for a thermally conductive filler that can provide a composition having excellent workability, thermal conductivity, and handling properties. DETAILED DESCRIPTION

[0037] One embodiment of the present invention is a siloxane compound represented by the following general formula (1):

[0038] [Chemistry 3]

[0039]

[0040] (Where R 1 , R 2 , R 3 , X, a, b and c are as defined above). It should be understood that: in the siloxane compound, R 1 Units, including R 2 Unit, SiR 3 The units shown in the formula (1) are not necessarily arranged as shown in the formula (1), and may be, for example, SiR 3 The unit shown in 2O exists in the 1 between the unit including R2.

[0041] It is believed that the siloxane compound having a cyclic structure represented by the general formula (1) can improve the processing efficiency of the thermally conductive filler because multiple hydrolyzable groups can be introduced into the cyclic structure and the hydrolyzable groups are concentrated in position, so the thermally conductive filler can be further highly filled. Moreover, since the above-mentioned siloxane compound itself has high heat resistance, it can impart high heat resistance to the thermally conductive polysiloxane composition. In addition, although not bound by a specific theory, it is believed that: by having a siloxane chain of appropriate length in the molecule, the distance between the part that interacts with the particles of the thermally conductive filler and the part that interacts with the silicone polymer can be appropriately controlled, and the inorganic particles as the thermally conductive filler and the silicone polymer as the base polymer can be appropriately played as a mediator, and the viscosity of the composition is reduced. Furthermore, there is the following advantage: such a siloxane compound can be easily obtained by, for example, allowing a cyclic siloxane containing a hydrogen group to react with a siloxane having a vinyl group at one end, or a silane compound containing a vinyl group and a hydrolyzable group.

[0042] In the general formula (1), R 1 It is a hydrolyzable functional group containing an alkoxysilyl group having 1 to 4 carbon atoms, and more specifically, groups having the following structures can be exemplified. 1 It can be bonded directly to X through silicon or through a linking group such as an ester bond. 1 , more specifically, groups having the following structures can be exemplified.

[0043] [Chemistry 4]

[0044]

[0045] Among them, from the perspective that the processing efficiency of the thermally conductive filler tends to be further improved, R 1 Preferably, it is a group having a structure of two or more, particularly three, alkoxysilyl groups. 1 It preferably contains a methoxysilyl group.

[0046] R 2 It is a group represented by the general formula (2).

[0047] [Chemistry 5]

[0048]

[0049] (Where R 4 , Y and d are as defined above).

[0050] In the general formula (2), the number of d is in the range of 10 to 50, preferably in the range of 10 to 40, and more preferably in the range of 20 to 30. By setting it in this range, the effect on fluidity is improved, high compounding is possible, the viscosity of the siloxane compound itself can be suppressed, and the stability is further improved. 4 Each of them is independently a monovalent hydrocarbon group having 1 to 12 carbon atoms, and examples thereof include: a linear or branched C 1-12 Alkyl; aryl such as phenyl and naphthyl. In addition, it may be substituted by halogen such as chlorine, fluorine, bromine, etc. As such a group, perfluoroalkyl such as trifluoromethyl can be exemplified. From the perspective of easy synthesis, R 4 A methyl group is preferred. Y is a monovalent hydrocarbon group having 1 to 6 carbon atoms. From the viewpoint of easy synthesis, Y is preferably a methyl group.

[0051] R 1 and R 2 The siloxane is bonded to the cyclic siloxane moiety of the siloxane represented by the general formula (1) via the group X. The group X is a divalent hydrocarbon group having 2 to 10 carbon atoms, and examples thereof include -CH2CH2-, -CH2CH2CH2-, -CH2CH2CH2CH2CH2CH2-, -CH2CH(CH3)-, and -CH2CH(CH3)CH2-, and other alkylene groups. From the perspective of ease of synthesis, X is preferably -CH2CH2- or -CH2CH(CH3)-.

[0052] R 3 Each R is independently a monovalent hydrocarbon group having 1 to 6 carbon atoms. 3 From the perspective of ease of synthesis, R 3 Preferred is methyl.

[0053] a is an integer greater than or equal to 1, preferably 1. b is an integer greater than or equal to 1, preferably 1 or 2. The value of b is preferably designed together with the value of d so that -SiR 4 The number of 2O- units is in the range of 20 to 60. c is an integer greater than or equal to 0, and preferably is from 0 to 2. The sum of a+b+c is an integer greater than or equal to 4, and is preferably 4 from the viewpoint of ease of synthesis.

[0054] As a representative example of the siloxane compound described above, there can be mentioned a compound represented by the following structural formula, but the present invention is not limited to this compound.

[0055] [Chemistry 6]

[0056]

[0057] Here, when describing the structure of a siloxane compound, the structural units of the siloxane compound may be described using the following abbreviations (hereinafter, these structural units may also be referred to as "M unit", "D unit", etc., respectively).

[0058] M:-Si(CH3)3O 1 / 2

[0059] M H :-SiH(CH3)2O 1 / 2

[0060] M Vi :-Si(CH=CH2)(CH3)2O 1 / 2

[0061] D:Si(CH3)2O 2 / 2

[0062] D H :SiH(CH3)O 2 / 2

[0063] T:Si(CH3)O 3 / 2

[0064] Q:SiO 4 / 2

[0065] For example, in the above general formula (2), R 4 The structure where Y is methyl and vinyl can be represented as -D n M vi However, it should be understood that, for example, H 20 D 20 When it is not 20 consecutive D H The meaning of this unit is that there are 20 consecutive D units after it, and the units can be arranged in any order.

[0066] The siloxane compound of the present invention can be prepared by a person skilled in the art using a known method or a similar method. As an example, a cyclic siloxane having two or more Si-H bonds is reacted with an alkoxysilane containing an unsaturated bond such as vinyltrimethoxysilane, and then reacted with a linear polysiloxane having an unsaturated bond, thereby obtaining a siloxane having a structure represented by the general formula (1). A person skilled in the art can appropriately select reaction conditions, purification methods, etc.

[0067] One embodiment of the present invention is a surface treatment agent for a thermally conductive filler containing the above-mentioned siloxane compound. The siloxane compound of the present invention functions as a surface treatment agent for a thermally conductive filler, and by mixing the surface-treated thermally conductive filler with a silicone polymer as a base polymer, a thermally conductive composition with excellent handling properties can be provided. The thermally conductive filler and the silicone polymer contained in the composition are described below.

[0068] [Thermal conductive filler]

[0069] As the thermally conductive filler, generally known inorganic fillers can be exemplified, and examples thereof include aluminum oxide, magnesium oxide, zinc oxide, boron nitride, aluminum nitride, silicon dioxide powder, silicon carbide, metal powder, diamond, aluminum hydroxide, carbon, etc. Aluminum oxide, zinc oxide, aluminum nitride, or silicon carbide is particularly preferred. As these inorganic fillers, there are no particular restrictions as long as they are of a grade that can be used as a thermally conductive filler, and commercially available products can be used.

[0070] The average particle size of the thermally conductive filler is not particularly limited as long as it is of an available grade, but preferably a thermally conductive filler having an average particle size of 300 μm or less is used. Among thermally conductive fillers having an average particle size within this range, if a large average particle size is added, the filling rate cannot be increased, and on the other hand, when the average particle size is small, the viscosity tends to increase. However, by appropriately selecting the average particle size of the thermally conductive filler and adding it, a composition with a viscosity that meets the target can be obtained.

[0071] In the thermal conductive filler, it is also preferred to use a filler with a relatively large particle size in combination with a filler with a relatively small particle size. By using a filler with a plurality of particle sizes in combination, the filler with a relatively small particle size enters the gap between the fillers with a relatively large particle size, thereby enabling further high filling. The filler can be divided into a large particle size (for example, a particle size of 30 μm or more), a medium particle size (for example, a particle size of 1 μm or more and less than 30 μm), and a small particle size (for example, a particle size less than 1 μm) according to the average particle size, and it is preferred to use at least two or more of these, especially three. When a plurality of fillers with different particle sizes are used, their mixing ratio can be set to any ratio. From the perspective of the operability of preparing the composition and the thermal conductivity of the obtained composition, it is preferred to use a filler with a large particle size of 30 to 70% by mass, and more preferably 35 to 65% by mass. When three fillers with a large particle size, a medium particle size, and a small particle size are used, the mixing ratio of the fillers with a medium particle size and a small particle size is preferably set in the range of 1:40 to 40:1, and more preferably in the range of 1:7 to 7:1.

[0072] There is no particular restriction on the shape of the inorganic particles used in the thermally conductive filler. For example, any of spherical, circular, and amorphous particles can be used, and at least two of these particles can be used in combination. The average particle size when the shape of the inorganic particles is circular or amorphous is defined by a person skilled in the art based on a known method. The average particle size can be obtained in the form of a weight average value (or median particle size) using a particle size distribution measuring device such as a laser diffraction method.

[0073] The amount of the filler in the thermally conductive polysiloxane resin is in the range of 10 to 5000 parts by mass, preferably 50 to 4000 parts by mass, more preferably 100 to 3000 parts by mass, based on 100 parts by mass of the total amount of the siloxane compound and the polysiloxane resin having a curable functional group. The effects of the present invention can be significantly exhibited when the amount is in the range of 10 to 5000 parts by mass, more preferably 100 to 3000 parts by mass.

[0074] [Silicone polymer]

[0075] The thermally conductive polysiloxane composition of the present invention contains a polyorganosiloxane resin as an organosilicon polymer, which is a base polymer. As a polyorganosiloxane resin, as long as it is a substance used as a matrix of silicone grease, silicone rubber, etc., linear, branched, cyclic polyorganosiloxane resins and the like can be used without particular limitation on their structure. In addition, modified silicones introduced with functional groups can also be used. For example, for the purpose of changing the hardness of the grease, the polyorganosiloxane resin can have one or more curable functional groups that become reaction sites for the curing reaction. Here, in this specification, "curable functional group" refers to a functional group that can participate in the curing reaction of the resin. Examples of curable functional groups include: vinyl, (meth) acryloyl, hydrogen groups directly bonded to silicon, etc. From the viewpoint of curability, these curable functional groups are preferably 2 or more in one molecule, and from the perspective of ease of acquisition or preparation, preferably 2 in one molecule. However, compounds having one curable functional group in one molecule can also be used. In addition, a plurality of compounds having different numbers of curable functional groups may be used in combination. The mechanism of the curing reaction is not particularly limited, and a method generally used for curing resins, such as an addition reaction and a condensation reaction, may be employed.

[0076] Examples of polysiloxane resins having curable functional groups that are cured by addition reaction include, but are not limited to, linear polyorganosiloxanes containing aliphatic unsaturated groups represented by the following general formula (3):

[0077] [Chemistry 7]

[0078]

[0079] (Where,

[0080] R a are independently, an aliphatic unsaturated group,

[0081] R are independently 1-6 Alkyl or C 6-12 Aryl,

[0082] n is a number that makes the viscosity at 23° C. 0.01 to 50 Pa·s. Among these linear polyorganosiloxanes, those in which R is all methyl and R is preferably used from the viewpoint of availability. a A polyorganosiloxane such as a vinyl group.

[0083] The amount of the polysiloxane resin having a curable functional group is preferably in the range of 1 to 50 parts by mass, more preferably in the range of 3 to 40 parts by mass, relative to 100 parts by mass of the thermally conductive filler. By setting it in this range, a uniform thermally conductive polysiloxane composition can be obtained without impairing the high thermal conductivity of the thermally conductive filler.

[0084] Polysiloxane resins can be classified according to curing reaction mechanisms such as addition reaction curing type and condensation reaction curing type. When classified according to the reaction mechanism, addition reaction curing type polysiloxane is preferably used from the viewpoint of productivity and operability. As addition reaction curing type polysiloxane, there is known an addition reaction curing type polysiloxane containing (a) an unsaturated group-containing polyorganosiloxane as a base polymer, (b) a hydrogen group-containing polyorganosiloxane as a crosslinking agent, and (c) a platinum compound as a curing catalyst.

[0085] The polyorganosiloxane containing unsaturated groups as component (a) preferably contains at least an average of 0.5 unsaturated groups in the organic group bonded to the silicon atom in one molecule. If the number of unsaturated groups in each molecule is less than 0.5, the components that do not participate in crosslinking increase, so a sufficient cured product cannot be obtained. If the number of unsaturated groups in each molecule is 0.5 or more, a cured product can basically be obtained, but if the number is too much, the heat resistance of the cured product decreases and the original purpose cannot be achieved, so it is preferably in the range of 0.5 to 2.0. From the perspective of easy preparation of polyorganosiloxane, the unsaturated group is preferably a vinyl group. The unsaturated group can be bonded to the end of the molecular chain, the side end of the molecular chain, or any position, but from the perspective of increasing the curing speed and maintaining the heat resistance of the cured product, it is preferably located at the end of the molecular chain.

[0086] As other functional groups in the polyorganosiloxane containing an unsaturated group, monovalent substituted or unsubstituted hydrocarbon groups can be listed, and examples thereof include alkyl groups such as methyl, ethyl, propyl, butyl, hexyl, and dodecyl; aryl groups such as phenyl; aralkyl groups such as 2-phenylethyl and 2-phenylpropyl; substituted hydrocarbon groups such as chloromethyl and 3,3,3-trifluoropropyl, etc. Methyl and phenyl are preferred from the perspective of ease of synthesis.

[0087] The structure of the unsaturated group-containing polyorganosiloxane may be either linear or branched. The viscosity thereof is not particularly limited, but is preferably 0.01 to 50 Pa·s at 23°C.

[0088] Generally, polyorganosiloxane containing unsaturated groups can be prepared by reacting hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, tetravinyltetramethylcyclotetrasiloxane and other cyclic siloxanes with R3SiO 0.5 The polysiloxane is obtained by equilibrium polymerization of an organosiloxane having a plurality of (here, R is a monovalent hydrocarbon group) units, followed by a neutralization step and removal of the remaining low-molecular siloxane component.

[0089] The hydrogen-containing polyorganosiloxane of component (b) is a siloxane compound having Si-H bonds and is a component that serves as a crosslinking agent. The amount of the polyorganosiloxane is such that the number of hydrogen atoms directly bonded to silicon atoms reaches 0.2 to 5.0 relative to one unsaturated group of component (a). If it is less than 0.2, curing will not proceed sufficiently, and if it exceeds 5.0, the cured product will become hard and the physical properties after curing will be adversely affected. In addition, the number of hydrogen groups bonded to silicon atoms contained in one molecule must be at least 2, and there are no special restrictions on other conditions, organic groups other than hydrogen groups, bonding positions, degree of polymerization, structure, etc., and two or more hydrogen-containing polyorganosiloxanes may also be used.

[0090] The hydrogen group-containing polyorganosiloxane typically has two or more units represented by the general formula (4) in the molecule.

[0091] (R b ) x (R c ) y SiO (4-x-y) / 2 (4)

[0092] (Where,

[0093] R b is a hydrogen atom,

[0094] R c C 1-6 Alkyl (e.g., methyl, ethyl, propyl, butyl, pentyl, hexyl, preferably methyl) or phenyl;

[0095] x is 1 or 2;

[0096] y is an integer from 0 to 2, wherein x+y is 1 to 3).

[0097] Examples of the siloxane skeleton in the hydrogen group-containing polyorganosiloxane include cyclic, branched, and linear skeletons, and a cyclic or branched skeleton is preferred.

[0098] The platinum compound of component (c) is a curing catalyst for reacting the unsaturated group of component (a) with the hydrogen group of component (b) to obtain a cured product. Examples of the platinum compound include chloroplatinic acid, platinum-olefin complexes, platinum-vinylsiloxane complexes, platinum-phosphorus complexes, platinum-alcohol complexes, platinum black, and the like. The amount of the compound is such that the amount reaches 0.1 to 1000 ppm in terms of platinum element relative to the polyorganosiloxane containing unsaturated groups of component (a). If it is less than 0.1 ppm, it will not be fully cured, and even if it exceeds 1000 ppm, a significant increase in the curing speed cannot be expected. In addition, in order to obtain a longer pot life, the activity of the catalyst can be suppressed by adding a reaction inhibitor. As known reaction inhibitors for platinum group metals, alkynols such as 2-methyl-3-butyn-2-ol and 1-ethynyl-2-cyclohexanol; and diallyl maleate.

[0099] As a method for preparing a composition containing a thermally conductive filler, a siloxane compound, a polysiloxane resin and a thermally conductive filler can be directly prepared using a mixing device, or the siloxane compound and the filler are first mixed and surface treated, and then dispersed in the polysiloxane resin. In addition, heating, decompression or other known methods can be applied as needed. In addition, in the case of containing the addition reaction curing polyorganosiloxane described above, a resin composition containing the above-mentioned component (a) can also be prepared in advance, and a mixture of components (b) and (c) can be added just before curing.

[0100] The amount of the siloxane compound represented by the general formula (1) in the thermally conductive composition is in the range of 0.01 to 20 parts by mass relative to 100 parts by mass of the thermally conductive filler. By setting the amount of the siloxane compound to this range, the filling property of the thermally conductive filler can be improved and the thermal conductivity can be improved. The amount of the siloxane compound is more preferably in the range of 0.1 to 15 parts by mass. In addition, it is preferably used in an amount of 1 part by mass or more relative to 100 parts by mass of the polysiloxane resin that becomes the base polymer. When the amount of the siloxane compound is less than 1 part by mass relative to the polysiloxane resin, the surface treatment effect of the thermally conductive filler is weakened and cannot be highly mixed. In addition, when excessive, it will have an adverse effect on the mechanical properties and heat resistance after curing, so it is more preferably in the range of 0.1 to 500 parts by mass.

[0101] The thermally conductive polysiloxane composition of the present invention may contain pigments, flame retardants, adhesion-imparting agents, heat resistance-imparting agents, diluents, organic solvents, etc. known to those skilled in the art as needed within a range not impairing the effects of the present invention.

[0102] When the polysiloxane resin has a curable functional group, the thermally conductive polysiloxane composition of the present invention can be cured to form a silicone rubber. The curing reaction of the polysiloxane composition can be performed by a method appropriately selected according to the type of the curable functional group of the polysiloxane resin.

[0103] When a polyorganosiloxane having a functional group such as an epoxy group that undergoes a curing reaction by heat is used as a curable functional group, the thermally conductive polysiloxane composition can also be cured by heating. The conditions for heat curing are well known to those skilled in the art, and as equipment that can be used in the heat curing reaction, for example, a thermostatic bath and other devices well known to those skilled in the art can be cited. The heating conditions can be appropriately adjusted according to the heat-resistant temperature of the parts to which the composition is applied, and the curing time can be determined. For example, heat of 40 to 100°C can be applied within a range of 1 minute to 5 hours. From the viewpoint of operability, the heating temperature is preferably 50 to 90°C, more preferably 60 to 80°C. From the viewpoint of the simplicity of the curing process, the heating time is preferably 5 minutes to 3 hours, more preferably 10 minutes to 2 hours.

[0104] The silicone rubber obtained by curing the thermally conductive polysiloxane composition of the present invention can be used as a heat dissipation member of electronic components such as electronic equipment and integrated circuit elements.

[0105] Example

[0106] Examples of the present invention are shown below, but the present invention is not limited to these examples. In the following examples and comparative examples, parts are all parts by mass.

[0107] Synthesis of materials

[0108] [Example 1]

[0109] Cyclic siloxane compound having a polysiloxane chain with a degree of polymerization of 20

[0110] [Chemistry 8]

[0111]

[0112] In a 5000 mL flask, 1100 g of vinyltrimethoxysilane was added to a solution of 440 g of toluene and 1992 g of a cyclic siloxane having two Si-H bonds in the presence of a platinum catalyst. The mixture was reacted at 120° C. for 3 hours. The solvent was removed from the obtained reaction solution and distilled to obtain a colorless liquid.

[0113] To 75 g of the obtained liquid, a linear vinyl polysiloxane (MD 20 M vi The polysiloxane shown: 300 g of Momentive) was further added with a platinum catalyst and reacted at 120° C. for 5 hours to obtain the target siloxane as a colorless oil.

[0114] FT IR was used to measure the -1 An absorption peak derived from the methoxy group was confirmed near 1 In H NMR measurement (500 MHz, CDCl3), a signal derived from a methoxy group was observed at 3.55 ppm, and based on the integral ratio with the signal derived from a methyl group adjacent to silicon at around 0.01 ppm, it was confirmed that a linear polysiloxane structure with about 20 D units was introduced into each molecule. In the results of GPC measurement, a monodisperse peak (dispersity 1.13) was confirmed, and the measured average molecular weight showed good consistency with the structural formula.

[0115] [Example 2]

[0116] Cyclic siloxane compound having a polysiloxane chain with a degree of polymerization of 30

[0117] [Chemistry 9]

[0118]

[0119] To 77 g of the liquid obtained in Example 1 as a reaction product of cyclic siloxane and vinyltrimethoxysilane, a linear vinyl polysiloxane (MD 30 M vi The polysiloxane shown: 450 g (produced by MOMENTIVE) was further added with a platinum catalyst and reacted at 120° C. for 5 hours to obtain the target siloxane as a colorless oil.

[0120] FT IR was used to measure the -1 An absorption peak derived from the methoxy group was confirmed near 1 In H NMR measurement (500 MHz, CDCl3), a signal derived from a methoxy group was observed at 3.56 ppm, and based on the integral ratio with the signal derived from a methyl group adjacent to silicon at around 0.04 ppm, it was confirmed that a linear polysiloxane structure with about 30 D units was introduced into each molecule. In the results of GPC measurement, a monodisperse peak (dispersity 1.15) was confirmed, and the measured average molecular weight showed good consistency with the structural formula.

[0121] [Example 3]

[0122] Cyclic siloxane compound having a polysiloxane chain with a degree of polymerization of 40

[0123] [Chemistry 10]

[0124]

[0125] The MD of the linear vinyl polysiloxane 30 M Vi The polysiloxane shown is changed to MD 40 M vi The reaction was completed and the target siloxane was obtained by the same method as in Example 2 except that the polysiloxane shown was obtained. 1 The results were confirmed by H NMR, FT IR and GPC measurements.

[0126] [Example 4]

[0127] Cyclic siloxane compound (2) having a polysiloxane chain with a degree of polymerization of 30

[0128] [Chemistry 11]

[0129]

[0130] The cyclic siloxane was replaced with a siloxane having three Si-H bonds, and MD, which is a linear vinyl polysiloxane, was used in an amount twice as large as that of the linear vinyl polysiloxane. 30 M Vi The reaction was completed and the target siloxane was obtained by the same method as in Example 1 except that the polysiloxane shown was obtained. 1 The results were confirmed by H NMR, FT IR and GPC measurements.

[0131] [Comparative Example 1]

[0132] Cyclic siloxane compound having a polysiloxane chain with a degree of polymerization of 70

[0133] [Chemistry 12]

[0134]

[0135] Vinyl trimethoxysilane was replaced with 3-(methacryloyloxy)propyl trimethoxysilane, and MD as a linear vinyl polysiloxane was used. 30 M vi The polysiloxane shown is changed to MD 70 M vi The reaction was completed and the target siloxane was obtained by the same method as in Example 4 except that the polysiloxane shown was obtained. 1 The results were confirmed by H NMR, FT IR and GPC measurements.

[0136] [Comparative Example 2]

[0137] Cyclic siloxane compound having a polysiloxane chain with a degree of polymerization of 200

[0138] [Chemistry 13]

[0139]

[0140] The MD of the linear vinyl polysiloxane 30 M Vi The polysiloxane shown is changed to MD 200 M vi The reaction was completed and the target siloxane was obtained by the same method as in Example 1 except that the polysiloxane shown was obtained. 1 The results were confirmed by H NMR, FT IR and GPC measurements.

[0141] The materials used in the following formulation examples and formulation comparative examples are as described above.

[0142] <Thermal Conductive Filler>

[0143] Round alumina with an average particle size of 0.4 μm (Sumicorundum AA-04: manufactured by Sumitomo Chemical)

[0144] <Polyorganosiloxane resin>

[0145] A,ω-divinyl polydimethylsiloxane; viscosity 0.35Pa·s

[0146] <Surface treatment agent: siloxane compound represented by general formula (1)>

[0147] The siloxanes obtained in Examples 1 to 4 and Comparative Examples 1 to 2 were used in each of Compounding Examples 1 to 4 and Compounding Comparative Examples 1 to 2. The correspondence between the Examples and Comparative Examples and the Compounding Examples and Comparative Compounding Examples is shown in Table 1. Hereinafter, the "polymerization number" indicates the number of -Si(CH3)2O contained in the siloxane compound. 2 / 2 - Total number of cells (D cells).

[0148] <<Curing Composition>>

[0149] <Polyorganosiloxane containing unsaturated groups>

[0150] α,ω-divinyl polydimethylsiloxane; viscosity 0.35Pa·s

[0151] α-Vinyl polydimethylsiloxane; viscosity 0.35Pa·s

[0152] <Hydrogen group-containing polyorganosiloxane>

[0153] MD H 20 D 20 M represents organohydrogen polysiloxane: viscosity 0.03 Pa·s

[0154] M H D 20 M H The organohydrogen polysiloxane shown: viscosity 0.02 Pa·s

[0155] <Platinum Catalyst>

[0156] Pt-M Vi M vi Complex (Platinum 1,2-divinyltetramethyldisiloxane complex)

[0157] <Reaction Inhibitor>

[0158] Diallyl maleate (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0159] [Surface treatment of aluminum oxide with siloxane compounds]

[0160] Matching Example A

[0161] 1 part by mass of each of the siloxane compounds of Formula Examples 1 to 4 and Comparative Formula Examples 1 to 2 as the siloxane compound represented by the general formula (1), a predetermined amount of α,ω-divinylpolydimethylsiloxane (viscosity 0.35 Pa·s) or α-vinylpolydimethylsiloxane (viscosity 0.35 Pa·s) as the polyorganosiloxane resin, and 100 parts by mass of Sumicorundum AA-04 as the alumina were kneaded by a planetary mixer by a predetermined method to obtain a thermally conductive polysiloxane composition A in which the alumina was surface-treated. The viscosity of the obtained composition A was measured at 23° C. using a rotary viscometer (VISMETRON VDH) (manufactured by Shibaura Systems Co., Ltd.) using a No. 7 rotor at 10 rpm for 1 minute in accordance with JIS K6249. The results are shown in Table 1.

[0162] Matching Example B

[0163] To 66.65 parts by weight of the thermally conductive polysiloxane composition A prepared in Formulation Example A, 4.5 parts by weight of α,ω-divinylpolydimethylsiloxane (viscosity 0.35 Pa·s) as a polyorganosiloxane containing an unsaturated group and the above-mentioned platinum-vinylsiloxane complex in an amount in which the catalyst concentration is 2 ppm in terms of platinum atoms are added. Furthermore, to the remaining 66.65 parts by weight of the thermally conductive polysiloxane composition A, MD as a polyorganosiloxane containing a hydrogen group is added. H 20 D20 M0.7 parts by mass and M H D 20 M H 1.06 parts by mass and 0.002 parts by mass of diallyl maleate as a reaction inhibitor were mixed separately by a planetary mixer by a prescribed method to obtain thermally conductive polysiloxane compositions B-1 and B-2. The obtained compositions B-1 and B-2 were mixed and stirred uniformly in a prescribed ratio, injected into an aluminum mold coated with Teflon (registered trademark) with an internal size of 6 mm (depth) × 60 mm (length) × 30 mm (width), and cured at 70°C for 30 minutes using a hot air circulation dryer. After the cured product was cooled to 23°C, the Type E hardness was measured based on JIS K6249. In addition, the thermal conductivity of the cured product was measured using TPS1500 (Kyoto Electronics Industry Co., Ltd.). In addition, the polysiloxane compositions B-1 and B-2 were placed in an environment of 70°C for 3 days, cooled to 23°C, and then B-1 and B-2 were mixed in a prescribed ratio and stirred evenly, and then injected into an aluminum mold coated with Teflon (registered trademark) with an internal size of 6 mm (depth) × 60 mm (length) × 30 mm (width), and cured at 70°C for 30 minutes using a hot air circulation dryer. After the cured product was cooled to 23°C, the Type E hardness was measured based on JIS K6249. The results are shown in Table 1 below.

[0164] [Table 1]

[0165]

[0166] As shown in Table 1, by using a siloxane compound represented by the general formula (1) having a siloxane chain structure of an appropriate length based on a predetermined range of polymerization number as a surface treatment agent, a composition having a manageable viscosity and substantially unchanged hardness in an accelerated test and excellent stability can be obtained. On the other hand, when the siloxane compound represented by the general formula (1) is not used, the hardness of the composition decreases over time, resulting in problems in stability.

[0167] Industrial Applicability

[0168] The siloxane compound of the present invention can provide a thermally conductive polysiloxane composition having excellent fluidity and stability, and can therefore be widely and effectively used as a material for heat dissipation members of electronic components such as various electronic devices and integrated circuit elements.

Claims

1. A method for producing a thermally conductive polysiloxane composition, comprising: A step of mixing a siloxane compound represented by the following general formula (1) with a thermally conductive filler to perform surface treatment; as well as, The step of dispersing the surface-treated thermally conductive filler in a polysiloxane resin, The amount of the siloxane compound is in the range of 0.01 to 1 parts by mass relative to 100 parts by mass of the thermally conductive filler. In formula (1), R 1 : A group having an alkoxysilyl group having 1 to 4 carbon atoms R 2 : A linear organic siloxy group represented by the following general formula (2) In formula (2), R 4 are each independently a monovalent hydrocarbon group having 1 to 12 carbon atoms, Y is a monovalent hydrocarbon group having 1 to 6 carbon atoms, d is an integer of 10 to 50, X: Each independently represents a divalent hydrocarbon group having 2 to 10 carbon atoms a and b: each independently an integer greater than 1 c: integer greater than 0 a+b+c: integer greater than 4 R 3 : Each independently represents a monovalent hydrocarbon group having 1 to 6 carbon atoms.

2. The method according to claim 1, wherein: In the general formula (1), b is 2 and d is 10-40.

3. The method according to claim 1, wherein: In the general formula (1), b is 1.