Wind power blade protective coating and preparation process thereof

Through the combination of polyether modified epoxy resin, acrylate copolymer and nanotitanium dioxide, the problem of insufficient adhesion, wear resistance and weather resistance of wind power blade coatings in extreme environments is solved, and efficient and long-lasting protection is formed Coating extends the service life of wind blades and reduces maintenance costs.

CN118931314APending Publication Date: 2024-11-12HENAN MAIWEI NEW MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411113586.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing wind power blade protective coatings have problems such as poor adhesion, poor wear resistance and insufficient weather resistance in extreme environments, resulting in coating peeling, wear and protection performance degradation, increasing maintenance frequency and cost.

Method used

The polyether modified epoxy resin, acrylate copolymer, silane coupling agent and nanotitanium dioxide are used to form a coating with high adhesion, wear resistance and aging resistance through high-speed dispersion and three-roller grinding process. Combining environmentally friendly solvents and curing agents, optimize the viscosity and curing conditions of the coating.

Benefits of technology

It achieves the durable stability and efficient protection of the coating, extends the service life of wind power blades, reduces maintenance frequency and operating costs, and improves the protection effect in environments such as salt spray, ultraviolet rays and sand and dust.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931314A_ABST
    Figure CN118931314A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of coatings, in particular to a wind power blade protective coating and a preparation process thereof. The invention relates to a wind power blade protective coating, which comprises polyether modified epoxy resin, an acrylate copolymer, a curing agent, a silane coupling agent, nano titanium dioxide, an auxiliary agent and a pigment, the preparation method comprises the following steps: premixing the polyether modified epoxy resin and the acrylate copolymer, adding the silane coupling agent, the nano titanium dioxide, the auxiliary agent and the pigment, mixing, grinding and refining, and adding the curing agent before use to obtain the wind power blade protective coating. Through raw material formula design and an optimized preparation process, the prepared coating can resist erosion of various environments, adhesive force, wear resistance, aging resistance and the like of a coating are comprehensively improved, long-acting and reliable protection is provided for the wind turbine blade, and the wind turbine blade cannot be damaged even in extreme environments such as salt mist, ultraviolet rays, sand dust and temperature difference. And the excellent protection effect can be kept, the maintenance period of the wind power blade is effectively prolonged, and the operation cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of coatings, and in particular to a wind turbine blade protective coating and a preparation process thereof. Background Art

[0002] Wind turbine blades are key components of wind turbines. They are exposed to the outdoors for a long time and face the test of extreme weather conditions, including strong winds, ultraviolet radiation, sandstorms, hail, and salt spray corrosion in the marine environment. Therefore, the protective coating used on the surface of wind turbine blades must have excellent weather resistance, wear resistance, chemical resistance and good adhesion to protect the blades from environmental damage and extend their service life.

[0003] Most of the existing wind turbine blade protective coatings use epoxy resin or polyurethane systems. Although they can provide protection to a certain extent, the resin system has insufficient bonding strength between the coating and the substrate, and the coating is prone to blistering, stratification, or even peeling in complex environments. Secondly, facing the impact of high-speed particles such as wind, sand, and hail, the surface hardness and wear resistance of the existing coatings are insufficient, and the coating is easily worn, affecting the aerodynamic performance and appearance of the blades, while reducing the protective effect. In addition, long-term exposure to harsh conditions such as ultraviolet rays, temperature differences, and salt spray makes the coating prone to powdering, cracking, and fading, further leading to a decrease in protective performance and an increase in maintenance frequency and cost. Therefore, in view of the fact that existing coatings still have problems such as poor adhesion, poor wear resistance, and insufficient weather resistance, the present invention provides a wind turbine blade protective coating and a preparation process thereof to solve the above problems. Summary of the invention

[0004] In view of the deficiencies in the prior art, the object of the present invention is to provide a wind turbine blade protective coating and a preparation process thereof.

[0005] A wind turbine blade protective coating comprises a main agent and a curing agent, wherein the main agent is composed of the following raw materials in parts by weight: 50-60 parts of polyether modified epoxy resin, 25-35 parts of acrylate copolymer, 1.8-2.2 parts of silane coupling agent, 4.5-5.5 parts of nano titanium dioxide, 0.8-1.2 parts of leveling agent, 0.4-0.6 parts of defoaming agent, 1.3-1.7 parts of dispersant and 9-11 parts of pigment; the curing agent is 9-11 parts by weight of amine compound.

[0006] Furthermore, the polyether segment in the polyether-modified epoxy resin accounts for 10-15% of the total weight of the resin.

[0007] The introduction of polyether chain segment-modified epoxy resin improves the flexibility and weather resistance of the resin, allowing it to maintain good adhesion and mechanical strength under extreme environments. At the same time, the hydrophilicity of the polyether chain segment helps to improve the compatibility with the silane coupling agent and enhance the interface bonding between the filler and the resin.

[0008] Furthermore, the acrylate copolymer contains one or more of acrylate, methacrylate or acrylic acid.

[0009] By selecting acrylate copolymers containing weather-resistant monomers, including butyl acrylate, methyl methacrylate, etc., the coating's anti-ultraviolet aging performance and weather resistance are enhanced, so that the coating can still maintain good appearance and function during long-term exposure to outdoor environments.

[0010] Furthermore, the curing agent is an alicyclic amine compound.

[0011] Furthermore, the silane coupling agent is selected from one or more of a vinyl silane coupling agent, an epoxy silane coupling agent, and a methacryloxy silane coupling agent.

[0012] The use of silane coupling agent greatly improves the bonding strength between fillers such as nano-titanium dioxide and the resin matrix, ensuring the long-term stability and wear resistance of the coating.

[0013] Furthermore, the average particle size of the nano titanium dioxide is 1-10 nm.

[0014] The use of titanium dioxide with an average particle size of less than 100 nanometers not only provides efficient UV shielding, but also utilizes its photocatalytic properties to make the coating self-cleaning, reduce the adhesion of wind sand and pollutants, and reduce maintenance costs.

[0015] A preparation process of a wind turbine blade protective coating comprises the following steps: Step a) accurately weighing the polyether-modified epoxy resin and the acrylate copolymer, adding them into a high-speed disperser according to the formula ratio, and stirring and mixing them at a low speed of 300-600 rpm to obtain a premix; Step b) adding silane coupling agent, nano titanium dioxide, leveling agent, defoamer, dispersant and pigment in sequence, dispersing at a high speed of 1000-2000 rpm for 30 min-1 h to obtain a premix; Step c) transferring the premix to the feed port of a three-roll mill or a bead mill, and grinding the premix through the equipment to refine the pigment and other fillers to the nanometer level to obtain a finished coating; Step d) Before use, the curing agent and the finished coating are mixed according to the ratio of the formula, and stirred thoroughly to prepare a wind turbine blade protective coating; Step e) Check the viscosity of the paint before construction and adjust it with a thinner if necessary.

[0016] The nano-level grinding process of high-speed dispersion and three-roll mill or bead mill is adopted to ensure the uniform dispersion of fillers and additives, improve the flatness and glossiness of the coating, reduce coating defects such as orange peel effect and bubbles, and enhance the aesthetics and protective performance of the coating.

[0017] The curing agent is mixed with the main agent in proportion before use to ensure that the curing reaction occurs during construction and avoid shortening the activity period due to premature activation. At the same time, the amount of curing agent added is precisely controlled to ensure that the chemical reaction during the coating curing process is complete and improve the hardness and durability of the coating.

[0018] Furthermore, the diluent used to adjust the viscosity in step e) is an environmentally friendly solvent, including water or an alcohol solvent.

[0019] The beneficial effects achieved by the present invention are as follows: 1. The coating prepared by the present invention, through raw material formula design and optimized preparation process, can resist various environmental erosions, achieve comprehensive improvement in adhesion, wear resistance, aging resistance and other aspects of the coating, form a durable and stable protective layer, and provide long-term and reliable protection for wind turbine blades. Even in extreme environments such as salt spray, ultraviolet rays, sand and dust, temperature differences, etc., it can maintain excellent protection effects, effectively extend the maintenance cycle of wind turbine blades, and reduce operating costs.

[0020] 2. The present invention uses a stable chemical bond formed between a polyether-modified epoxy resin and the surface of a composite material, combined with the interface strengthening effect of a silane coupling agent, to significantly improve the adhesion between the coating and the substrate, ensure the long-term adhesion of the coating on the surface of a wind turbine blade, and reduce the risk of coating peeling and delamination caused by environmental factors.

[0021] 3. The present invention utilizes the synergistic effect of nano-titanium dioxide and acrylate copolymer to enhance the surface hardness and wear resistance of the coating, effectively resist high-speed impacts such as wind, sand, and hail, reduce wear and damage, and ensure the aerodynamic performance and appearance quality of wind turbine blades.

[0022] 4. The present invention uses a composite system of polyether modified epoxy resin and acrylate copolymer to provide excellent UV resistance and temperature change resistance, combined with the photocatalytic and UV absorption properties of nano titanium dioxide, greatly improving the aging resistance of the coating and ensuring the stability of the coating performance of wind turbine blades during long-term outdoor use.

[0023] 5. This aspect uses environmentally friendly solvents, water or alcohol solvents as diluents to reduce VOC emissions. At the same time, the viscosity adjustment and optimization of curing conditions before construction ensure the construction adaptability and curing effect of the coating in different environments, reduce the impact on the environment, and respond to the industry trend of green chemistry and sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1A schematic flow chart of a preparation process of a wind turbine blade protective coating used in an embodiment of the present invention; Figure 2 The formula of the wind turbine blade protective coating used in Examples 1 to 3 of the present invention; Figure 3 These are the test results of the drying time, adhesion, sagging performance, flexibility, impact resistance, tensile strength and elongation at break of the wind turbine blade protective coatings used in Examples 1 to 3 of the present invention and the comparative example; Figure 4 These are the test results of the acid resistance, alkali resistance, salt spray resistance, UV resistance and wear resistance of the wind turbine blade protective coatings used in Examples 1 to 3 of the present invention and the comparative example. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below in conjunction with specific embodiments.

[0026] Embodiment 1: A wind turbine blade protective coating, such as Figure 2 As shown, it includes a main agent and a curing agent, and the main agent is composed of the following raw materials in parts by weight: 55 parts of polyether modified epoxy resin (polyether segment accounts for 12% of the total weight of the resin), 30 parts of acrylate copolymer (acrylate-methacrylate copolymer), 2 parts of silane coupling agent KH550 (γ-aminopropyltriethoxysilane), 5 parts of nano titanium dioxide (average particle size 3nm), 1 part of leveling agent (organic silicone leveling agent BYK-306), 0.5 parts of defoaming agent (organic silicone defoaming agent BYK-052), 1.5 parts of dispersant (polymer dispersant BYK-190) and 10 parts of pigment (rutile titanium dioxide); 10 parts by weight of curing agent (EPIKURE Curing Agent 3240 (Huntsman product)) are used.

[0027] A preparation process of a wind turbine blade protective coating, such as Figure 1 As shown, the following steps are included: a) accurately weighing a polyether-modified epoxy resin and an acrylate copolymer, adding them into a high-speed disperser according to the formula ratio, and stirring and mixing them at a low speed of 450 rpm to obtain a premix; b) adding silane coupling agent, nano titanium dioxide, leveling agent, defoamer, dispersant and pigment in sequence, increasing the speed to 1500 rpm, and dispersing at medium-high speed for 45 minutes to obtain a premix; c) transferring the premix to the feed port of a three-roll mill, and grinding the premix through the equipment to refine the pigment and other fillers to the nanometer level to obtain a finished coating; d) Before use, mix the curing agent and the finished coating according to the formula ratio, stir them thoroughly and evenly to prepare the wind turbine blade protective coating; e) Check whether the viscosity of the coating is appropriate before construction, and adjust it with a thinner if necessary; f) Use high-pressure airless spraying to evenly apply paint on the surface of the wind turbine blade, and the dry film thickness of the spraying is controlled at 100μm; g) Curing naturally at room temperature, and the ambient temperature of the curing process is controlled at 25°C.

[0028] Embodiment 2: A wind turbine blade protective coating, such as Figure 2 As shown, it includes a main agent and a curing agent, and the main agent is composed of the following raw materials in parts by weight: 60 parts of polyether modified epoxy resin (polyether segment accounts for 10% of the total weight of the resin), 25 parts of acrylate copolymer (acrylate-methacrylate copolymer), 1.8 parts of silane coupling agent KH550 (γ-aminopropyltriethoxysilane), 4.5 parts of nano titanium dioxide (average particle size 5nm), 0.8 parts of leveling agent (organic silicone leveling agent BYK-306), 0.4 parts of defoaming agent (organic silicone defoaming agent BYK-052), 1.3 parts of dispersant (polymer dispersant BYK-190) and 9 parts of pigment (rutile titanium dioxide); 9 parts by weight of curing agent (EPIKURE Curing Agent 3240 (Huntsman product)) are used.

[0029] A preparation process of a wind turbine blade protective coating, such as Figure 1 As shown, the following steps are included: a) accurately weighing the polyether-modified epoxy resin and the acrylate copolymer, adding them into a high-speed disperser according to the formula ratio, and stirring and mixing them at a low speed of 350 rpm to obtain a premix; b) adding silane coupling agent, nano titanium dioxide, leveling agent, defoamer, dispersant and pigment in sequence, increasing the speed to 1200 rpm, and dispersing at medium-high speed for 55 minutes to obtain a premix; c) transferring the premix to the feed port of a bead mill, and grinding the premix through the equipment to refine the pigment and other fillers to the nanometer level to obtain a finished coating; d) Before use, mix the curing agent and the finished coating according to the formula ratio, stir them thoroughly and evenly to prepare the wind turbine blade protective coating; e) Before construction, check whether the viscosity of the paint is appropriate and adjust it with thinner if necessary.

[0030] f) Use air spraying to evenly apply paint on the surface of the wind turbine blade, and the dry film thickness of the spraying is controlled at 100μm; g) Curing naturally at room temperature, and the ambient temperature of the curing process is controlled at 25°C.

[0031] Embodiment 3: A wind turbine blade protective coating, such as Figure 2As shown, it includes a main agent and a curing agent, and the main agent is composed of the following raw materials in parts by weight: 50 parts of polyether modified epoxy resin (polyether segment accounts for 15% of the total weight of the resin), 35 parts of acrylate copolymer (acrylate-acrylic acid copolymer), 2.2 parts of silane coupling agent A-174 (γ-methacryloxypropyltrimethoxysilane), 5.5 parts of nano titanium dioxide (average particle size 10nm), 1.2 parts of leveling agent (organic silicon leveling agent BYK-306), 0.6 parts of defoaming agent (organic silicon defoaming agent BYK-052), 1.7 parts of dispersant (polymer dispersant BYK-190) and 11 parts of pigment (rutile titanium dioxide); 11 parts by weight of curing agent (dicyandiamide) are used.

[0032] A preparation process of a wind turbine blade protective coating, such as Figure 1 As shown, the following steps are included: a) accurately weighing a polyether-modified epoxy resin and an acrylate copolymer, adding them into a high-speed disperser according to the formula ratio, and stirring and mixing them at a low speed of 550 rpm to obtain a premix; b) adding silane coupling agent, nano titanium dioxide, leveling agent, defoamer, dispersant and pigment in sequence, increasing the speed to 1800 rpm, and dispersing at medium-high speed for 35 minutes to obtain a premix; c) transferring the premix to the feed port of a three-roll mill, and grinding the premix through the equipment to refine the pigment and other fillers to the nanometer level to obtain a finished coating; d) Before use, mix the curing agent and the finished coating according to the formula ratio, stir them thoroughly and evenly to prepare the wind turbine blade protective coating; e) Before construction, check whether the viscosity of the paint is appropriate and adjust it with thinner if necessary.

[0033] f) Use high-pressure airless spraying to evenly apply paint on the surface of the wind turbine blade, and the dry film thickness of the spraying is controlled at 100μm; g) Curing naturally at room temperature, and the ambient temperature of the curing process is controlled at 25°C.

[0034] Comparative Example: Compared with Example 1, this comparative example uses unmodified epoxy resin and pure acrylate copolymer, and does not use silane coupling agent and nano titanium dioxide, and other conditions are consistent with Example 1; The wind turbine blade protective coating comprises a main agent and a curing agent, wherein the main agent is composed of the following raw materials in parts by weight: 55 parts of epoxy resin, 30 parts of acrylate copolymer (pure acrylate copolymer), 1 part of leveling agent (silicone leveling agent BYK-306), 0.5 parts of defoamer (silicone defoamer BYK-052), 1.5 parts of dispersant (polymer dispersant BYK-190) and 10 parts of pigment (rutile titanium dioxide); 10 parts by weight of curing agent (EPIKURE Curing Agent 3240 (Huntsman product)) was used.

[0035] The preparation process of wind turbine blade protective coating comprises the following steps: a) Accurately weigh epoxy resin and acrylate copolymer, add them into a high-speed disperser according to the formula ratio, and stir and mix them at a low speed of 450 rpm to obtain a premix; b) adding leveling agent, defoamer, dispersant and pigment in sequence, increasing the speed to 1500 rpm, and dispersing at medium-high speed for 45 minutes to obtain a premix; c) transferring the premix to the feed port of a three-roll mill, and grinding the premix through the equipment to refine the pigment and other fillers to the nanometer level to obtain a finished coating; d) Before use, the curing agent and the finished coating are mixed according to the ratio of the formula, and stirred thoroughly to obtain the wind turbine blade protective coating; e) Check whether the viscosity of the coating is appropriate before construction, and adjust it with a thinner if necessary; f) Use high-pressure airless spraying to evenly apply paint on the surface of the wind turbine blade, and the dry film thickness of the spraying is controlled at 100μm; g) Curing naturally at room temperature, and the ambient temperature of the curing process is controlled at 25°C.

[0036] It should be noted that: In addition to the actual selections embodied in the above specific embodiments, the weight ratio of the polyether-modified epoxy resin to the acrylate copolymer is feasible in the range of 40-60:40-60, and the weight ratio of the polyether-modified epoxy resin to the curing agent is feasible in the range of 80-90:10-20. Through the appropriate ratio, the crosslinking density, flexibility and strength are balanced; In addition to the actual selections embodied in the above specific embodiments, the leveling agent can be selected from existing silicone leveling agents, such as BYK Chemical's leveling agent series, Evonik Degussa's TEGO Glide series, SH 8400, etc. Those skilled in the art can adaptably select from existing raw materials according to needs; In addition to the actual selections embodied in the above specific embodiments, the defoamer can be selected from existing silicone defoamers, such as BYK Chemical's defoamer series, 272s of Uka Chemical, and 245s of Uka Chemical. Those skilled in the art can adaptably select from existing raw materials according to needs; In addition to the actual selections embodied in the above specific embodiments, the dispersant may be an existing polymer dispersant, such as UCAR 510s, UCAR 568s, UCAR 615s, etc., and those skilled in the art may adaptably select from the existing raw materials according to their needs; In addition to the actual selections embodied in the above specific embodiments, the pigment can be selected from one or more combinations of titanium dioxide, limestone powder, bentonite, talc, precipitated barium sulfate, barite powder, mica powder, feldspar powder and wollastonite powder, and the particle size is within the range of 800-1250 mesh; In addition to the actual selections embodied in the above specific embodiments, the method of applying coating on the surface of wind turbine blades may be electrostatic spraying, powder spraying, brushing, rolling, dipping, rotary cup spraying, etc., and technical personnel in this field can make adaptive selections according to needs.

[0037] Test Example: Relevant performance tests were performed on the wind turbine blade protective coatings prepared in Examples 1 to 3 and the comparative examples; 1. Drying time: GB / T 1728-2020 Determination of drying time of paint film and putty film The experimental temperature is 23±2℃, and the relative humidity is 50±5%. Metal plates with sizes and materials that meet the test standards are selected as substrates to ensure that they are clean, grease-free and dust-free. A standard coater (wire rod coater) is used to evenly coat the wind turbine blade protective coating on the metal plate with a thickness of 100μm. Time is recorded immediately after coating is completed. At regular intervals, use a clean finger to gently touch the coating surface. When the finger touches the surface and no traces or adhesion are left, it is recorded as the surface drying time. After the surface is dry, continue to monitor the curing of the coating. With the help of a cross-cutting device, when the coating can withstand slight pressure without deformation and there is no coating peeling in the cross-cutting test, the coating can be considered to be completely hardened, which is recorded as the complete drying time.

[0038] 2. Adhesion: GB / T 5210-2006 Adhesion test of paint and varnish by pull-off method Use a standard coater to evenly coat the wind turbine blade protective coating on the metal plate with a thickness of 100μm. After it is completely dried and cured, use a grid cutter to make a grid on the coating surface. The blade of the grid cutter is perpendicular to the surface of the substrate. Apply force evenly during cutting to ensure that the cutting depth of each grid penetrates the coating directly to the substrate. The standard grid size is 2mm×2mm. After cutting, use a soft brush to gently remove debris in the grid area, stick a piece of tape on the top of the grid area, ensure that the tape fits tightly to the coating, press the tape to make it fully contact with the coating, and then quickly tear off the tape at an angle close to 90°. Carefully observe the grid area and evaluate the degree of peeling of the coating. Evaluate the adhesion level of the coating from level 0 (no peeling) to level 5 (complete peeling).

[0039] 3. Sagging performance: GB / T 5210 Same as test 2 The wind turbine blade protective coating is applied on the vertical surface of the metal plate with a thickness of 100 μm. After the coating is completed, the metal plate is immediately kept in a vertical position to observe whether the coating begins to sag under the action of gravity and record the degree of sagging. The degree of sagging is expressed by measuring the size of the sagging area.

[0040] 4. Flexibility: GB / T 1731-2020 Determination of paint film flexibility Select a metal rod that meets the standards as the substrate, ensure that its surface is clean, oil-free and rust-free, use a standard applicator to evenly apply the wind turbine blade protective coating on the metal rod with a thickness of 100μm, and fully dry and cure at room temperature. Place the coated metal rod on the axis of a bending device with a diameter of 1mm, and then slowly bend the metal rod to subject the coating to bending stress, with a bending angle of 180°. After bending, carefully check the surface of the coating to observe whether there are cracks, peeling or other forms of damage to evaluate flexibility.

[0041] 5. Impact resistance: GB / T 1732-2020 Determination of impact resistance of coating films Use a standard coater to evenly coat the wind turbine blade protective coating on the metal plate with a thickness of 100μm. After fully drying and curing at room temperature, place the coated metal plate under the impact tester, set the drop height of the heavy hammer to 50cm, release the heavy hammer and let it fall freely to the coating surface. After the impact, carefully check the surface of the coating to see if there are cracks, peeling or any other form of damage, and evaluate the impact resistance.

[0042] 6. Tensile strength: ISO527-3—2012 Determination of tensile properties of plastics Part 3: Test conditions for sheets, films and flat moldings The dry films formed by the final curing of Example 1, Example 2, Example 3 and the comparative example were cut into a rectangle of 100 mm×150 mm, and placed at a temperature of 23±2° C. and a relative humidity of 50±5% for 24 hours. The dry films were clamped between the upper and lower clamps of a tensile testing machine to ensure that the length (gauge length) of the sample between the clamps met the standard requirements. The tensile testing machine was started to stretch the sample at a constant speed (1 mm / min to 500 mm / min) until the sample broke. During the stretching process, the tensile force exerted on the sample and the deformation length of the sample were recorded in real time. When the sample broke, the maximum tensile force value at the moment of breaking and the total deformation length of the sample were recorded. The tensile strength was calculated by the formula, that is, the maximum tensile force value divided by the original cross-sectional area of ​​the sample. 7. Elongation at break: ISO527-3 Same as test 6 According to the test results of Experiment 6, the elongation at break was calculated by the formula, which is the percentage of the deformation length of the specimen at break to the original gauge length.

[0043] 8. Acid resistance: GB / T 9274-1988 Determination of resistance of paints and varnishes to liquid media The dry films formed by curing of Example 1, Example 2, Example 3 and the comparative example were selected as samples, cut into squares of 100 mm × 100 mm, and 5% by mass dilute sulfuric acid was prepared. The samples were completely immersed in the prepared dilute sulfuric acid solution for 24 hours. After the immersion, the samples were carefully taken out from the solution, and the surfaces of the samples were thoroughly cleaned with clean water to remove the residual solution. The samples were then placed in a well-ventilated place to dry naturally. After drying, the appearance changes of the coating were carefully observed and recorded, including whether there were color changes, blistering, peeling, cracks or other damages. Based on the observation results, the acid resistance of the coating was evaluated.

[0044] 9. Alkali resistance: GB / T 9274 Same as test 8 The dry films formed by curing of Example 1, Example 2, Example 3 and the comparative example were selected as samples, cut into squares of 100 mm × 100 mm, and a potassium hydroxide solution with a mass fraction of 5% was prepared. The samples were completely immersed in the prepared potassium hydroxide solution for 24 hours. After the immersion, the samples were carefully taken out from the solution, and the surfaces of the samples were thoroughly cleaned with clean water to remove the residual solution. The samples were then placed in a well-ventilated place to dry naturally. After drying, the appearance changes of the coating were carefully observed and recorded, including whether there were color changes, blistering, peeling, cracks or other damages. Based on the observation results, the alkali resistance of the coating was evaluated.

[0045] 10. Salt spray resistance: GB / T 1771-2007 Determination of neutral salt spray resistance of paints and varnishes The dry films finally formed by curing of Example 1, Example 2, Example 3 and the comparative example were cut into rectangles of 100 mm × 150 mm as samples. A 5% sodium chloride solution was prepared with pure water as a water source for generating salt spray. A salt spray chamber was used to generate a salt spray with a pH value of about 7.0. The temperature in the chamber was maintained at 35±2° C. The samples were placed horizontally in the salt spray chamber to ensure that the surface of the samples was in direct contact with the salt spray. The salt spray chamber was opened to expose the samples to the salt spray environment for 168 hours (7 days). After the test, the samples were carefully removed from the salt spray chamber, and the surface of the samples was rinsed with warm water to remove residual salt spray deposits. Subsequently, the samples were placed in a well-ventilated place to dry naturally. After drying, the coating surface was carefully inspected to assess whether there was rust, peeling, discoloration or other forms of corrosion. Based on the observation results, the salt spray resistance of the coating was assessed.

[0046] 11. UV resistance: GB / T 14522-2008 Test methods for artificial weathering of plastics, coatings and rubber materials for mechanical industrial products The dry films of Example 1, Example 2, Example 3 and the comparative example were selected as coating samples. An ultraviolet aging box equipped with ultraviolet lamps in a specific wavelength range and a humidity and temperature control system was used to simulate ultraviolet radiation in nature to simulate real environmental conditions. According to the test requirements, a light cycle was set, including an illumination stage and a condensation or spraying stage, to simulate the sunlight during the day and the influence of humidity at night. The samples were fixed on the bracket in the ultraviolet aging box to ensure that the surface of the sample maintained a certain distance from the light source to obtain uniform lighting. The ultraviolet aging box was started to expose the sample to simulated ultraviolet rays for 600 hours. During the test, the color change, gloss reduction, powdering, cracking or blistering of the coating were recorded. After the test was completed, the changes of the sample before and after the test were compared to evaluate the ultraviolet resistance of the coating.

[0047] 12. Abrasion resistance: GB / T 1768-2006 Determination of abrasion resistance of paint and varnish films The dry films of Example 1, Example 2, Example 3 and the comparative example were cut into a circle with a diameter of 70 mm as a sample. Before the test, the initial weight of the sample was accurately weighed and recorded. Using an abrasion tester, the load of the friction head was set to 800 g and the number of frictions was set to 800 times. The sample was fixed on a rotating table to ensure that the surface of the sample was in good contact with the friction head. The abrasion tester was started to rub the friction head on the surface of the sample for a predetermined number of times. The sample was weighed again and the weight after the test was recorded. The weight loss of the coating was obtained by calculating the weight difference of the sample before and after the test to evaluate the wear degree and morphology of the coating.

[0048] The above performance test results are as follows Figure 3 and Figure 4 As shown, it can be seen that compared with the comparative example, the wind turbine blade protective coatings prepared in Examples 1 to 3 have better adhesion, wear resistance and weather resistance.

[0049] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A wind turbine blade protective coating, characterized in that: The invention comprises a main agent and a curing agent, wherein the main agent is composed of the following raw materials in parts by weight: 50-60 parts of polyether modified epoxy resin, 25-35 parts of acrylate copolymer, 1.8-2.2 parts of silane coupling agent, 4.5-5.5 parts of nano titanium dioxide, 0.8-1.2 parts of leveling agent, 0.4-0.6 parts of defoaming agent, 1.3-1.7 parts of dispersant and 9-11 parts of pigment; and the curing agent is 9-11 parts by weight of amine compound.

2. A wind turbine blade protective coating according to claim 1, characterized in that: The polyether segments in the polyether-modified epoxy resin account for 10-15% of the total weight of the resin.

3. The wind turbine blade protective coating according to claim 1, characterized in that: The acrylate copolymer contains one or more of acrylate, methacrylate or acrylic acid.

4. The wind turbine blade protective coating according to claim 1, characterized in that: The curing agent is an alicyclic amine compound.

5. The wind turbine blade protective coating according to claim 1, characterized in that: The silane coupling agent is selected from one or more of a vinyl silane coupling agent, an epoxy silane coupling agent, and a methacryloxy silane coupling agent.

6. The wind turbine blade protective coating according to claim 1, characterized in that: The average particle size of the nano titanium dioxide is 1-10 nm.

7. The preparation process of a wind turbine blade protective coating according to claim 1, characterized in that: The following steps are involved: Step a) accurately weighing the polyether-modified epoxy resin and the acrylate copolymer, adding them into a high-speed disperser according to the formula ratio, and stirring and mixing them at a low speed of 300-600 rpm to obtain a premix; Step b) adding silane coupling agent, nano titanium dioxide, leveling agent, defoamer, dispersant and pigment in sequence, dispersing at a high speed of 1000-2000 rpm for 30 min-1 h to obtain a premix; Step c) transferring the premix to the feed port of a three-roll mill or a bead mill, and grinding the premix through the equipment to refine the pigment and other fillers to the nanometer level to obtain a finished coating; Step d) Before use, the curing agent and the finished coating are mixed according to the ratio of the formula, and stirred thoroughly to prepare a wind turbine blade protective coating; Step e) Check the viscosity of the paint before construction and adjust it with a thinner if necessary.

8. The preparation process of a wind turbine blade protective coating according to claim 7, characterized in that: The diluent used to adjust the viscosity in step e) is an environmentally friendly solvent, including water or an alcohol solvent.

Citation Information

Patent Citations

  • Solventless two-component quick-drying anti-corrosion coating and production method

    CN109161302A

  • Nanometer solvent-free epoxy anticorrosive paint and preparation method thereof

    CN111087894A

  • High-salt-spray-resistance and high-weather-resistance two-component water-based primer-topcoat coating and preparation method thereof

    CN114806330A