Water-based porcelain coating and preparation method thereof
By fixing the aminosilane coupling agent on the surface of the ceramic microspheres and combining it with aqueous epoxy resin, the problem of insufficient dispersion and interface bonding ability of ceramic powder in the coating is solved, and the impact resistance of ceramic coatings is significantly improved. Stain resistance and gloss stability.
Patent Information
- Application Number
- CN202411192611.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
AI Technical Summary
Existing porcelain coatings have shortcomings in the surface modification of ceramic microspheres, resulting in poor dispersion of ceramic powders in the material and weak interface bonding ability, affecting the gloss, hardness and scrubbing resistance of the coating.
The ceramic microspheres are modified by surface-fixed aminosilane coupling agent to retain the reactivity of siloxane groups and amino groups. The ceramic microspheres are prepared by spray drying and sintering, and are then combined with aqueous epoxy in the coating. The resin and other ingredients combine to form a high-performance aqueous porcelain coating.
It significantly improves the dispersion of ceramic microspheres in the organic system and the ability to combine with other materials, improves the impact resistance, water resistance, salt resistance and stain resistance of the coating. The pencil hardness reaches 4H and the scrubbing resistance exceeds that of 20,000 times, the gloss change has good stability.
Smart Images

Figure BDA0005015502370000241 
Figure HDA0005015502390000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water-based coatings, and in particular relates to a water-based porcelain coating and a preparation method thereof. Background Art
[0002] With the massive construction of national highways, the mileage of tunnel construction has increased significantly. The brightness and uniformity of tunnel lighting and road lighting have affected the driving safety of vehicles. At present, the decorative materials used in tunnels usually adopt paving tiles or industrial coatings to solve the above problems. Although tiles can improve the illumination, due to the humid environment in the tunnel, the walls often seep and crack, and there is a great risk of tiles falling off; industrial coatings have average reflective effects. At the same time, the coating surface is easy to be contaminated, maintenance is difficult, and the reflective effect is easy to deteriorate.
[0003] In response to the special needs of the inner wall of the tunnel, porcelain coatings (or porcelain coatings, ceramic coatings), especially organic-inorganic composite porcelain coatings, have been gradually developed and applied. Porcelain coatings are a kind of imitation porcelain glaze coatings. After the construction is completed, a decorative coating similar to a ceramic surface will appear on the surface of the building. Its main characteristics are high hardness and not easy to be scratched; good reflective performance and high brightness; corrosion resistance, stain resistance, and easy cleaning. In addition to the inner wall of the tunnel, it is also widely used on the surfaces of various other cement or metal structures.
[0004] The invention patent application (202310003002.5) discloses an environmentally friendly and easy-to-clean tunnel high-gloss porcelain coating and its preparation method, including high-hydroxy polyurethane emulsion, high modulus silica sol, isocyanate curing agent and other fillers and additives. The cross-linking reaction of high-hydroxy polyurethane emulsion and isocyanate curing agent is the main method, and high modulus silica sol powder is introduced. During this process, the hydroxyl group and the isocyanate group react with each other, and the silica sol molecules are interspersed and riveted to each other to form the final high-gloss coating. The gloss meets the requirements of high gloss at 85° angle and relatively low gloss at 60° angle (gloss at 60° angle 10.1, gloss at 85° angle ≥60). Polyurethane materials have high flexibility, but they are lacking in coating hardness, especially in terms of scrub resistance. Even through the blending modification of silica sol molecules, it is difficult to have a substantial improvement. Therefore, the research on porcelain coatings is more based on epoxy resins with higher hardness, and coatings with higher hardness and better scrub resistance have been obtained.
[0005] The invention patent application (202111571661.6) discloses a high-strength porcelain coating and its preparation method, including water-based synthetic resin, hydrophobic reflective microbeads, water-based polyurethane and other fillers and additives, and the surface of the reflective microbeads is treated with a silane coupling agent to be hydrophobic, thereby further improving the hydrophobicity of the coating itself. This application mainly hydrophobizes the luminous microbeads, and the technical solution is more similar to traditional reflective coatings. Loose reflective microspheres cannot significantly improve the gloss, hardness and other aspects of the coating.
[0006] The invention patent application (201910427121.7) discloses a water-based epoxy resin porcelain coating, including water-based epoxy resin, water-based epoxy resin curing agent, ceramic powder, aluminum oxide dispersion and other pigments and fillers. The application discloses that in the process of preparing the curing agent, the epoxy-terminated silicone is grafted onto the curing agent molecule, and the epoxy resin molecules, curing agent molecules, and epoxy-terminated silicone molecules in the epoxy resin emulsion form a whole. The silicon atoms on the organic polymer will combine with the filler, the silicon atoms in the auxiliary agent, the aluminum atoms and other inorganic materials, and the epoxy resin and the inorganic material are combined through the silicone functional group on the curing agent. The application does not clarify the beneficial effects of the modification of the curing agent molecules on the coating performance. The material as a whole is still a blended modification of various organic and inorganic materials, and it does not clarify the specific improvements in the final coating in terms of gloss, hardness, etc.
[0007] The existing ceramic coatings are mostly modified by blending organic and inorganic materials. The optimization of the formula is mainly aimed at the selection and modification of organic resins, but the modification of the key component of the material, the ceramic powder, is less, which makes it difficult to make a breakthrough in the performance of the molding material. The research on ceramic powder is mainly reflected in the surface modification of ceramics. The surface properties of micron-sized inorganic powder materials such as ceramic powders and ceramic microspheres are very different from those of polymer organic systems, which also makes it difficult for inorganic powders to be well dispersed in the material. Therefore, when inorganic powders are added to polymer composite materials, the surface of the inorganic powders must first be modified to make the surface of the particles organic, improve its lipophilicity and compatibility with the matrix, enhance the interface bonding ability, and thus play the function of the inorganic powders. The relevant modification methods are roughly divided into the following six types: 1. Surface coverage modification; 2. Chemical coating modification; 3. Precipitation reaction modification; 4. Mechanical chemical reaction; 5. External film layer modification; 6. High energy surface modification.
[0008] Chemical coating modification is a common modification method that uses chemical reactions to make organic molecules adsorb to the surface of ceramic powders and then coat the ceramic powders, so that the surface of the powder particles has new functions. Hu Xuehui used tartaric acid, EDTA, and sodium D-gluconate as chelating agents to modify barium titanate ceramics in "Preparation and Dielectric Properties of 0-3 Modified Ceramic / Polymer Composite Materials" to study the dielectric properties of modified ceramic materials. Chelating agents can react with metal atoms on the surface of ceramics to form cyclic chelates, among which chelating agents are multidentate ligand complexing agents and are widely used in metallurgy and oilfield descaling. The results show that: first, the effect of interface modification increases with the increase of barium titanate content. When the volume fraction of modified barium titanate is high, the interface modification effect is obvious and the dielectric constant increases more; secondly, the chelate layer acting between the inorganic phase and the organic phase improves the interface connection, which is beneficial to the dispersibility of the inorganic phase, thereby improving the dielectric constant of the system.
[0009] In chemical coating modification, the most commonly used is the surface grafting polymerization coating method, which is to connect the polymer material to the surface of the inorganic particle through chemical reaction. The characteristic of this method is that the polymer modifier that is finally grafted and coated on the modified body is synthesized simultaneously during the modification process. For example, when silicon carbide powder is treated with an organic silicon coupling agent, the organic monomer is grafted on the particle surface through polymerization reaction under suitable conditions to form a polyelectrolyte layer. The dispersion stability of the modified silicon carbide powder in water is much better than that of the unmodified silicon carbide powder.
[0010] The Chinese invention patent application (CN202311256558.1) discloses "A method for modifying ceramic powder, microwave dielectric ceramic slurry, preparation method and application thereof". The application adopts an organic coating method to modify the surface function of ceramic powder, that is, a multifunctional acrylate monomer containing a siloxane group is used, one end of which contains an acrylate group that can participate in the photopolymerization reaction, and the other end contains a siloxane group. The siloxane group can be grafted on the surface of the ceramic powder after hydrolysis, and the acrylate group grafted on the surface of the ceramic powder is exposed, so that the ceramic powder has a photosensitive property. The photosensitive group can undergo a polymerization reaction with the acrylate group in the photosensitive resin used in the ceramic slurry to improve the curing performance of the ceramic slurry.
[0011] The grafting modification of silane coupling agent and ceramic materials depends on the hydroxyl groups on the ceramic surface to form -Si-O- chemical bonds. Wang Xing showed in "Research on the Application of Silane Coupling Agent in Porcelain Repair" that under acidic catalytic conditions, hydrolyzed silane molecules are prone to condensation reactions to form siloxane oligomers, and these siloxane oligomer molecules can continue to condense to form polysiloxane compounds with linear or even network structures. It is generally believed that after the hydrolysis of silane coupling agent, most of the monomers and a small amount of oligomers in the hydrolyzate play a coupling role. If most of the monomer components in the hydrolyzate condense, it is bound to affect the effectiveness of the coupling agent; on the other hand, the hydrolysis reaction of the silane coupling agent introduces organic functional groups on the ceramic powder, which also loses the activity of the siloxane groups on the silane coupling agent.
[0012] In summary, the technical problem to be solved by the present invention is to modify and fix the silane coupling agent on the surface of the inorganic material in the porcelain coating, that is, the ceramic microspheres, and retain the reactivity of the two reactive groups on the silane coupling agent, that is, the siloxane group (inorganic group) and the amino group (organic group), so as to compound a water-based porcelain coating with better application performance. Summary of the invention
[0013] In order to solve the above technical problems, the present invention provides a water-based porcelain coating.
[0014] The technical solution adopted by the present invention is: a water-based porcelain paint, the composition and content of which are as follows by mass:
[0015] Component A: 47-55 parts of water-based epoxy resin emulsion;
[0016] Component B: 47-55 parts of waterborne epoxy resin curing agent, 25-22 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 10-5 parts of precipitated barium sulfate, 9-11 parts of rutile titanium dioxide, 0.5-0.1 parts of defoaming agent, 0.4-0.2 parts of brightening and leveling agent, 0.4-0.2 parts of anti-sagging agent, 0.5-0.3 parts of thickener, and 7.2-6.2 parts of water;
[0017] The specific preparation method of the ceramic microspheres with aminosilane coupling agent fixed on the surface is as follows:
[0018] The first step is slurry preparation
[0019] 45-50 parts of calcined kaolin with a particle size of 30-50 nm, 10-25 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 45-25 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 0.3-1.3 parts of a dispersant are added, and after ball milling and mixing for 1.5 hours, 0.3-1.5 parts of a binder are added, and the ball milling and mixing is continued for 2-4 hours to obtain a slurry;
[0020] The second step is spray drying
[0021] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 8000-25000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0022] The third step is microsphere sintering
[0023] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0024] Step 4: Surface modification
[0025] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 1 to 2.5 parts of a first catalyst having a particle size of 30 to 50 nm, silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening, the reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours;
[0026] Step 5: Alcoholysis
[0027] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 30 to 75 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are filtered to obtain the ceramic microspheres, the reaction temperature is 60 to 70° C., and the reaction time is 4 hours;
[0028] Step 6: Addition reaction
[0029] The ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and 10 to 25 parts of 3-chloropropylene are subjected to an addition reaction under the action of 1 to 2.5 parts of a second catalyst with a particle size of 30 to 50 nm, and the hydrogen-containing alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropyl alkoxysilane, and the ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0030] Step 7: Ammonolysis
[0031] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor, and subjected to aminolysis reaction with 20 to 50 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate aminosilane coupling agent. The reaction temperature is 85 to 95°C. After the reaction is completed, the ceramic microspheres with aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5 hours.
[0032] Step 8: Preparation of water-based porcelain paint
[0033] Mix 47-55 parts of waterborne epoxy resin curing agent in component B, 25-22 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 10-5 parts of precipitated barium sulfate, 9-11 parts of rutile titanium dioxide, 0.5-0.1 parts of defoaming agent, 0.4-0.2 parts of gloss enhancing and leveling agent, 0.4-0.2 parts of anti-sagging agent, 0.5-0.3 parts of thickener, and 7.2-6.2 parts of water evenly;
[0034] Then, the evenly mixed mixture of component B is evenly mixed with 47 to 55 parts of the water-based epoxy resin emulsion of component A to obtain a water-based porcelain coating.
[0035] A further preferred embodiment: the dispersant is any one of tetramethylammonium hydroxide, sodium hexametaphosphate, polyacrylate, citrate, and sodium humate.
[0036] A further preferred embodiment: the binder is any one of sodium carboxymethyl cellulose, methyl cellulose, polyvinyl alcohol, polypropylene, saccharin, dextrin, starch and gum arabic.
[0037] A further preferred embodiment: the first catalyst is any one of a copper-based catalyst and an iron-based catalyst.
[0038] A further preferred embodiment: the alcoholysis agent is any one of methanol and ethanol.
[0039] A further preferred embodiment: the second catalyst is hydrated ruthenium trichloride.
[0040] A further preferred embodiment: the defoamer, gloss enhancing and leveling agent, anti-sagging agent and thickener are all water-soluble compounds.
[0041] The preparation method of the water-based porcelain coating of the present invention is completed according to the following method:
[0042] The first step is to uniformly mix 47-55 parts of a waterborne epoxy resin curing agent, 25-22 parts of ceramic microspheres with an aminosilane coupling agent fixed on the surface, 10-5 parts of precipitated barium sulfate, 9-11 parts of rutile titanium dioxide, 0.5-0.1 parts of a defoaming agent, 0.4-0.2 parts of a gloss-enhancing leveling agent, 0.4-0.2 parts of an anti-sagging agent, 0.5-0.3 parts of a thickener, and 7.2-6.2 parts of water to obtain component B;
[0043] The second step is to mix component B and component A composed of 47 to 55 parts of water-based epoxy resin emulsion to obtain a water-based porcelain coating.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] First, the aminosilane coupling agent is fixed on the surface of the ceramic microspheres, and the reactivity of the two reactive groups on the silane coupling agent, the siloxane group (inorganic group) and the amino group (organic functional group), is retained. The retained amino group can react with other organic materials, while the retained siloxane group can combine with other inorganic materials.
[0046] Second, the aminosilane coupling agent fixed on the surface of ceramic microspheres can effectively help the ceramic material to be evenly and stably dispersed in the organic system; it can also effectively combine with the organic and inorganic substances in the material, so that the ceramic microspheres can effectively form a whole with other materials.
[0047] Third, while ensuring excellent performance in terms of impact resistance, water resistance, salt resistance, etc., the pencil hardness of the present invention can reach 4H, while the pencil hardness of general porcelain coatings can reach 2H; the scrub resistance can reach more than 20,000 times, while the scrub resistance of general porcelain coatings is generally required to reach more than 10,000 times; there is also a significant improvement in stain resistance and stain resistance durability.
[0048] Fourth, in terms of stain resistance, the present invention has a comprehensive stain resistance (60° gloss value) that is basically stable at more than 80, and is a high-gloss coating (generally, coatings with a 60° gloss value of >60 are called high-gloss coatings), and has a good light reflection effect. The absolute value of the gloss change difference is stable at 0.7-0.8, while the absolute value of the gloss change difference of general porcelain coatings is stable at 2-3, and the absolute value of the gloss change difference of general coatings is stable at about 5, indicating that the water-based porcelain coating of the present application has good stain resistance, and pollution and scrubbing operations have little effect on the gloss of the coating surface.
[0049] Fifth, in terms of stain resistance durability, the coating surface of the water-based porcelain coating of the present invention has a slightly decreased stain resistance (60° gloss value) after repeated pollution and scrubbing, but it is still above 80. The absolute value of the gloss change difference has increased steadily to about 1, but the absolute value of the gloss change difference of general porcelain coatings is stable at 3 to 4, and the absolute value of the gloss change difference of general coatings reaches more than 7, indicating that the water-based porcelain coating of the present application has good stain resistance durability, and repeated pollution and scrubbing operations have little effect on the gloss of the coating surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 These are infrared spectra of ordinary ceramic microspheres (a) and ceramic microspheres with aminosilane coupling agents fixed on their surfaces (b). DETAILED DESCRIPTION
[0051] Example 1
[0052] A water-based porcelain paint, the composition and content of which are as follows by mass:
[0053] Component A: 47 parts of water-based epoxy resin emulsion;
[0054] Component B: 47 parts of water-based epoxy resin curing agent, 25 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 10 parts of precipitated barium sulfate, 9 parts of rutile titanium dioxide, 0.5 parts of water-soluble defoaming agent, 0.4 parts of water-soluble brightening and leveling agent, 0.4 parts of water-soluble anti-sagging agent, 0.5 parts of water-soluble thickener, and 7.2 parts of water;
[0055] The specific preparation method of the ceramic microspheres with aminosilane coupling agent fixed on the surface is as follows:
[0056] The first step is slurry preparation
[0057] 45 parts of calcined kaolin with a particle size of 30-50 nm, 10 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 45 parts of deionized water are added to a ball mill, and after ball milling and mixing for 30 minutes, 0.3 parts of dispersant tetramethylammonium hydroxide are added, and after ball milling and mixing for 1.5 hours, 0.3 parts of binder sodium shuttle methyl cellulose are added, and the mixture is ball milled and mixed for 2 hours to obtain a slurry;
[0058] The second step is spray drying
[0059] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 22000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0060] The third step is microsphere sintering
[0061] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0062] Step 4: Surface modification
[0063] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 1 part of the first catalyst with a particle size of 30-50 nm, silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening, the reaction temperature is 350-450° C., the reaction pressure is 0.3-0.5 MPa, and the reaction time is 4 hours;
[0064] Step 5: Alcoholysis
[0065] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 30 to 75 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are filtered to obtain the ceramic microspheres, the reaction temperature is 60 to 70° C., and the reaction time is 4 hours;
[0066] Step 6: Addition reaction
[0067] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and an addition reaction is carried out with 10 parts of 3-chloropropylene in the presence of 1 part of a second catalyst with a particle size of 30 to 50 nm, the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropyl alkoxysilane, and the ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0068] Step 7: Ammonolysis
[0069] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to an aminolysis reaction with 20 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate an aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with the aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0070] The method of water-based porcelain coating described in this embodiment is completed as follows:
[0071] In the first step, 47 parts of waterborne epoxy resin curing agent, 25 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 10 parts of precipitated barium sulfate, 9 parts of rutile titanium dioxide, 0.5 parts of water-soluble defoaming agent, 0.4 parts of water-soluble gloss enhancing leveling agent, 0.4 parts of water-soluble anti-sagging agent, 0.5 parts of water-soluble thickener, and 7.2 parts of water are mixed uniformly to obtain component B;
[0072] In the second step, component B is mixed evenly with component A consisting of 475 parts of water-based epoxy resin emulsion to obtain a water-based porcelain coating.
[0073] Example 2
[0074] A water-based porcelain paint, the composition and content of which are as follows by mass:
[0075] Component A: 48 parts of water-based epoxy resin emulsion;
[0076] Component B: 48 parts of water-based epoxy resin curing agent, 24 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 9 parts of precipitated barium sulfate, 10 parts of rutile titanium dioxide, 0.4 parts of water-soluble defoaming agent, 0.3 parts of water-soluble brightening and leveling agent, 0.3 parts of water-soluble anti-sagging agent, 0.4 parts of water-soluble thickener, and 7 parts of water;
[0077] The specific preparation method of the ceramic microspheres with aminosilane coupling agent fixed on the surface is as follows:
[0078] A method for preparing ceramic microspheres with a particle size of 50 to 80 μm and an aminosilane coupling agent fixed on the surface:
[0079] The first step is slurry preparation
[0080] 46 parts of calcined kaolin with a particle size of 30-50 nm, 12 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 42 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 0.4 parts of dispersant sodium hexametaphosphate are added, and after ball milling and mixing for 1.5 hours, 0.4 parts of binder methyl cellulose are added, and the mixture is ball milled and mixed for 2.5 hours to obtain a slurry;
[0081] The second step is spray drying
[0082] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 15000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0083] The third step is microsphere sintering
[0084] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0085] Step 4: Surface modification
[0086] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 1.5 parts of a first catalyst having a particle size of 30 to 50 nm. Silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0087] Step 5: Alcoholysis
[0088] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 35 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are obtained by filtration, and the reaction temperature is 60-70° C. and the reaction time is 4 hours;
[0089] Step 6: Addition reaction
[0090] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and are subjected to an addition reaction with 15 parts of 3-chloropropylene in the presence of 1.5 parts of a second catalyst having a particle size of 30 to 50 nm, wherein the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropylalkoxysilane, and the ceramic microspheres with 3-chloropropylalkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0091] Step 7: Ammonolysis
[0092] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to an aminolysis reaction with 25 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate an aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with the aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0093] The method of water-based porcelain coating described in this embodiment is completed as follows:
[0094] In the first step, 48 parts of a water-based epoxy resin curing agent, 24 parts of ceramic microspheres with an aminosilane coupling agent fixed on the surface, 9 parts of precipitated barium sulfate, 10 parts of rutile titanium dioxide, 0.4 parts of a water-soluble defoaming agent, 0.3 parts of a water-soluble gloss-enhancing leveling agent, 0.3 parts of a water-soluble anti-sagging agent, 0.4 parts of a water-soluble thickener, and 7 parts of water are uniformly mixed to obtain component B;
[0095] In the second step, component B is mixed evenly with component A consisting of 48 parts of water-based epoxy resin emulsion to obtain a water-based porcelain coating.
[0096] Example 3
[0097] A water-based porcelain paint, the composition and content of which are as follows by mass:
[0098] Component A: 49 parts of water-based epoxy resin emulsion;
[0099] Component B: 49 parts of water-based epoxy resin curing agent, 23 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 8 parts of precipitated barium sulfate, 11 parts of rutile titanium dioxide, 0.3 parts of water-soluble defoaming agent, 0.2 parts of water-soluble brightening and leveling agent, 0.2 parts of water-soluble anti-sagging agent, 0.3 parts of water-soluble thickener, and 6.8 parts of water;
[0100] The specific preparation method of the ceramic microspheres with aminosilane coupling agent fixed on the surface is as follows:
[0101] A method for preparing ceramic microspheres with a particle size of 80 to 100 μm and an aminosilane coupling agent fixed on the surface:
[0102] The first step is slurry preparation
[0103] 47 parts of calcined kaolin with a particle size of 30-50 nm, 14 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 40 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 0.5 parts of dispersant polyacrylate are added, and after ball milling and mixing for 1.5 hours, 0.5 parts of binder gum arabic are added, and the mixture is ball milled and mixed for 2 hours to obtain a slurry;
[0104] The second step is spray drying
[0105] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 8000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0106] The third step is microsphere sintering
[0107] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0108] Step 4: Surface modification
[0109] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 1.7 parts of a first catalyst having a particle size of 30 to 50 nm. The silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0110] Step 5: Alcoholysis
[0111] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 32 parts of an alcoholysis agent under the protection of an inert gas, and the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, which is filtered to obtain ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface, the reaction temperature is 60-70° C., and the reaction time is 4 hours;
[0112] Step 6: Addition reaction
[0113] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and an addition reaction is carried out with 10 parts of 3-chloropropylene in the presence of 1.8 parts of a second catalyst with a particle size of 30 to 50 nm, and the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropyl alkoxysilane, and the ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0114] Step 7: Ammonolysis
[0115] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to an aminolysis reaction with 23 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate an aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with the aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0116] The method of water-based porcelain coating described in this embodiment is completed as follows:
[0117] In the first step, 49 parts of a water-based epoxy resin curing agent, 23 parts of ceramic microspheres with an aminosilane coupling agent fixed on the surface, 8 parts of precipitated barium sulfate, 11 parts of rutile titanium dioxide, 0.3 parts of a water-soluble defoaming agent, 0.2 parts of a water-soluble gloss-enhancing leveling agent, 0.2 parts of a water-soluble anti-sagging agent, 0.3 parts of a water-soluble thickener, and 6.8 parts of water are mixed uniformly to obtain component B;
[0118] In the second step, component B is mixed evenly with component A consisting of 49 parts of water-based epoxy resin emulsion to obtain a water-based porcelain coating.
[0119] The defoamer, gloss-enhancing and leveling agent, anti-sagging agent and thickener described in this embodiment are all water-soluble compounds.
[0120] Example 4
[0121] A water-based porcelain paint, the composition and content of which are as follows by mass:
[0122] Component A: 50 parts of water-based epoxy resin emulsion;
[0123] Component B: 50 parts of water-based epoxy resin curing agent, 22 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 7 parts of precipitated barium sulfate, 9 parts of rutile titanium dioxide, 0.2 parts of water-soluble defoaming agent, 0.4 parts of water-soluble brightening and leveling agent, 0.3 parts of water-soluble anti-sagging agent, 0.3 parts of water-soluble thickener, and 6.5 parts of water;
[0124] The specific preparation method of the ceramic microspheres with aminosilane coupling agent fixed on the surface is as follows:
[0125] A method for preparing ceramic microspheres with a particle size of 30 to 80 μm and an aminosilane coupling agent fixed on the surface:
[0126] The first step is slurry preparation
[0127] 48 parts of calcined kaolin with a particle size of 30-50 nm, 16 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 38 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 0.6 parts of dispersant citrate are added, and after ball milling and mixing for 1.5 hours, 0.6 parts of binder dextrin are added, and the ball milling and mixing is continued for 2.5 hours to obtain a slurry;
[0128] The second step is spray drying
[0129] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 8000-20000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0130] The third step is microsphere sintering
[0131] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0132] Step 4: Surface modification
[0133] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 1.3 parts of a first catalyst having a particle size of 30 to 50 nm. Silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0134] Step 5: Alcoholysis
[0135] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 35 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are obtained by filtration, and the reaction temperature is 60-70° C. and the reaction time is 4 hours;
[0136] Step 6: Addition reaction
[0137] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and are subjected to an addition reaction with 18 parts of 3-chloropropylene in the presence of 1.6 parts of a second catalyst having a particle size of 30 to 50 nm, wherein the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropylalkoxysilane, and the ceramic microspheres with 3-chloropropylalkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0138] Step 7: Ammonolysis
[0139] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to aminolysis reaction with 30 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0140] The method of water-based porcelain coating described in this embodiment is completed as follows:
[0141] In the first step, 50 parts of a water-based epoxy resin curing agent, 22 parts of ceramic microspheres with an aminosilane coupling agent fixed on the surface, 7 parts of precipitated barium sulfate, 9 parts of rutile titanium dioxide, 0.2 parts of a water-soluble defoaming agent, 0.4 parts of a water-soluble gloss-enhancing leveling agent, 0.3 parts of a water-soluble anti-sagging agent, 0.3 parts of a water-soluble thickener, and 6.5 parts of water are uniformly mixed to obtain component B;
[0142] In the second step, component B is mixed evenly with component A consisting of 50 parts of water-based epoxy resin emulsion to obtain a water-based porcelain coating.
[0143] Example 5
[0144] A water-based porcelain paint, the composition and content of which are as follows by mass:
[0145] Component A: 51 parts of water-based epoxy resin emulsion;
[0146] Component B: 51 parts of water-based epoxy resin curing agent, 25 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 6 parts of precipitated barium sulfate, 10 parts of rutile titanium dioxide, 0.1 parts of water-soluble defoaming agent, 0.3 parts of water-soluble brightening and leveling agent, 0.4 parts of water-soluble anti-sagging agent, 0.4 parts of water-soluble thickener, and 6.3 parts of water;
[0147] The specific preparation method of the ceramic microspheres with aminosilane coupling agent fixed on the surface is as follows:
[0148] A method for preparing ceramic microspheres with a particle size of 50 to 100 μm and an aminosilane coupling agent fixed on the surface:
[0149] The first step is slurry preparation
[0150] 49 parts of calcined kaolin with a particle size of 30-50 nm, 18 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 36 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 0.7 parts of dispersant sodium humate are added, and after ball milling and mixing for 1.5 hours, 0.8 parts of binder starch are added, and the mixture is ball milled and mixed for 2.5 hours to obtain a slurry;
[0151] The second step is spray drying
[0152] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 8000-12000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0153] The third step is microsphere sintering
[0154] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0155] Step 4: Surface modification
[0156] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 2 parts of a first catalyst having a particle size of 30 to 50 nm. The silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0157] Step 5: Alcoholysis
[0158] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 50 parts of an alcoholysis agent under the protection of an inert gas, and the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, which is filtered to obtain ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface, the reaction temperature is 60-70° C., and the reaction time is 4 hours;
[0159] Step 6: Addition reaction
[0160] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and are subjected to an addition reaction with 18 parts of 3-chloropropylene in the presence of 1.7 parts of a second catalyst having a particle size of 30 to 50 nm, wherein the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropylalkoxysilane, and the ceramic microspheres with 3-chloropropylalkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0161] Step 7: Ammonolysis
[0162] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to aminolysis reaction with 45 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0163] The method of water-based porcelain coating described in this embodiment is completed as follows:
[0164] In the first step, 51 parts of a water-based epoxy resin curing agent, 25 parts of ceramic microspheres with an aminosilane coupling agent fixed on the surface, 6 parts of precipitated barium sulfate, 10 parts of rutile titanium dioxide, 0.1 parts of a water-soluble defoaming agent, 0.3 parts of a water-soluble gloss-enhancing leveling agent, 0.4 parts of a water-soluble anti-sagging agent, 0.4 parts of a water-soluble thickener, and 6.3 parts of water are mixed uniformly to obtain component B;
[0165] In the second step, component B is mixed evenly with component A consisting of 51 parts of water-based epoxy resin emulsion to obtain a water-based porcelain coating.
[0166] Example 6
[0167] A water-based porcelain paint, the composition and content of which are as follows by mass:
[0168] Component A: 52 parts of water-based epoxy resin emulsion;
[0169] Component B: 52 parts of water-based epoxy resin curing agent, 24 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 5 parts of precipitated barium sulfate, 11 parts of rutile titanium dioxide, 0.1 parts of water-soluble defoaming agent, 0.2 parts of water-soluble brightening and leveling agent, 0.3 parts of water-soluble anti-sagging agent, 0.4 parts of water-soluble thickener, and 6.2 parts of water;
[0170] The specific preparation method of the ceramic microspheres with aminosilane coupling agent fixed on the surface is as follows:
[0171] A method for preparing ceramic microspheres with a particle size of 30 to 50 μm and an aminosilane coupling agent fixed on the surface:
[0172] The first step is slurry preparation
[0173] 50 parts of calcined kaolin with a particle size of 30-50 nm, 19 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 34 parts of deionized water are added into a ball mill, and after ball milling the mixture for 30 minutes, 0.8 parts of dispersant sodium humate are added, and after ball milling the mixture for 1.5 hours, 1.0 parts of binder polyvinyl alcohol are added, and the mixture is ball milled for 2.5 hours to obtain a slurry;
[0174] The second step is spray drying
[0175] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 25000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0176] The third step is microsphere sintering
[0177] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0178] Step 4: Surface modification
[0179] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 2.3 parts of a first catalyst having a particle size of 30 to 50 nm. Silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0180] Step 5: Alcoholysis
[0181] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 55 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are obtained by filtration, and the reaction temperature is 60-70° C. and the reaction time is 4 hours;
[0182] Step 6: Addition reaction
[0183] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and subjected to an addition reaction with 20 parts of 3-chloropropylene under the action of 2.4 parts of a second catalyst with a particle size of 30-50 nm, the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropyl alkoxysilane, and the ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70-80° C., and the reaction time is 4 hours;
[0184] Step 7: Ammonolysis
[0185] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to aminolysis reaction with 28 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0186] The method of water-based porcelain coating described in this embodiment is completed as follows:
[0187] In the first step, 52 parts of a water-based epoxy resin curing agent, 24 parts of ceramic microspheres with an aminosilane coupling agent fixed on the surface, 5 parts of precipitated barium sulfate, 11 parts of rutile titanium dioxide, 0.1 parts of a water-soluble defoaming agent, 0.2 parts of a water-soluble gloss-enhancing leveling agent, 0.3 parts of a water-soluble anti-sagging agent, 0.4 parts of a water-soluble thickener, and 6.2 parts of water are mixed uniformly to obtain component B;
[0188] In the second step, component B is mixed evenly with component A consisting of 52 parts of water-based epoxy resin emulsion to obtain a water-based porcelain coating.
[0189] Example 7
[0190] A water-based porcelain paint, the composition and content of which are as follows by mass:
[0191] Component A: 53 parts of water-based epoxy resin emulsion;
[0192] Component B: 53 parts of water-based epoxy resin curing agent, 23 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 8 parts of precipitated barium sulfate, 9 parts of rutile titanium dioxide, 0.2 parts of water-soluble defoaming agent, 0.4 parts of water-soluble brightening and leveling agent, 0.2 parts of water-soluble anti-sagging agent, 0.5 parts of water-soluble thickener, and 6.4 parts of water;
[0193] The specific preparation method of the ceramic microspheres with aminosilane coupling agent fixed on the surface is as follows:
[0194] A method for preparing ceramic microspheres with a particle size of 50 to 80 μm and an aminosilane coupling agent fixed on the surface:
[0195] The first step is slurry preparation
[0196] 49 parts of calcined kaolin with a particle size of 30-50 nm, 20 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 32 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 0.9 parts of dispersant citrate are added, and after ball milling and mixing for 1.5 hours, 1.2 parts of binder polypropylene are added, and the mixture is ball milled and mixed for 3 hours to obtain a slurry;
[0197] The second step is spray drying
[0198] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 17000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0199] The third step is microsphere sintering
[0200] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0201] Step 4: Surface modification
[0202] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 2.5 parts of a first catalyst having a particle size of 30 to 50 nm. The silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0203] Step 5: Alcoholysis
[0204] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 30 to 75 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are filtered to obtain the ceramic microspheres, the reaction temperature is 60 to 70° C., and the reaction time is 4 hours;
[0205] Step 6: Addition reaction
[0206] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and are subjected to an addition reaction with 19 parts of 3-chloropropylene in the presence of 2.3 parts of a second catalyst having a particle size of 30 to 50 nm, wherein the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropylalkoxysilane, and the ceramic microspheres with 3-chloropropylalkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0207] Step 7: Ammonolysis
[0208] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to aminolysis reaction with 48 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0209] The method of water-based porcelain coating described in this embodiment is completed as follows:
[0210] In the first step, 53 parts of a water-based epoxy resin curing agent, 23 parts of ceramic microspheres with an aminosilane coupling agent fixed on the surface, 8 parts of precipitated barium sulfate, 9 parts of rutile titanium dioxide, 0.2 parts of a water-soluble defoaming agent, 0.4 parts of a water-soluble gloss-enhancing leveling agent, 0.2 parts of a water-soluble anti-sagging agent, 0.5 parts of a water-soluble thickener, and 6.4 parts of water are mixed uniformly to obtain component B;
[0211] In the second step, component B is mixed evenly with component A consisting of 53 parts of water-based epoxy resin emulsion to obtain a water-based porcelain coating.
[0212] Example 8
[0213] A water-based porcelain paint, the composition and content of which are as follows by mass:
[0214] Component A: 54 parts of water-based epoxy resin emulsion;
[0215] Component B: 54 parts of water-based epoxy resin curing agent, 22 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 7 parts of precipitated barium sulfate, 10 parts of rutile titanium dioxide, 0.3 parts of water-soluble defoaming agent, 0.3 parts of water-soluble brightening and leveling agent, 0.3 parts of water-soluble anti-sagging agent, 0.3 parts of water-soluble thickener, and 6.6 parts of water;
[0216] The specific preparation method of the ceramic microspheres with aminosilane coupling agent fixed on the surface is as follows:
[0217] A method for preparing ceramic microspheres with a particle size of 80 to 100 μm and an aminosilane coupling agent fixed on the surface:
[0218] The first step is slurry preparation
[0219] 48 parts of calcined kaolin with a particle size of 30-50 nm, 22 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 30 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 1.0 part of a dispersant polyacrylate is added, and after ball milling and mixing for 1.5 hours, 1.3 parts of a binder dextrin is added, and the ball milling and mixing is continued for 3 hours to obtain a slurry;
[0220] The second step is spray drying
[0221] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 9000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0222] The third step is microsphere sintering
[0223] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0224] Step 4: Surface modification
[0225] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 2.1 parts of a first catalyst having a particle size of 30 to 50 nm. Silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0226] Step 5: Alcoholysis
[0227] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 65 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are obtained by filtration, and the reaction temperature is 60-70° C. and the reaction time is 4 hours;
[0228] Step 6: Addition reaction
[0229] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and subjected to addition reaction with 20 parts of 3-chloropropylene under the action of 1.4 parts of a second catalyst with a particle size of 30-50 nm, the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropyl alkoxysilane, and the ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70-80° C., and the reaction time is 4 hours;
[0230] Step 7: Ammonolysis
[0231] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor, and subjected to an aminolysis reaction with 19 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate an aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with the aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0232] The method of water-based porcelain coating described in this embodiment is completed as follows:
[0233] In the first step, 54 parts of a water-based epoxy resin curing agent, 22 parts of ceramic microspheres with an aminosilane coupling agent fixed on the surface, 7 parts of precipitated barium sulfate, 10 parts of rutile titanium dioxide, 0.3 parts of a water-soluble defoaming agent, 0.3 parts of a water-soluble gloss-enhancing leveling agent, 0.3 parts of a water-soluble anti-sagging agent, 0.3 parts of a water-soluble thickener, and 6.6 parts of water are mixed uniformly to obtain component B;
[0234] In the second step, component B is mixed evenly with component A consisting of 54 parts of water-based epoxy resin emulsion to obtain a water-based porcelain coating.
[0235] Example 9
[0236] A water-based porcelain paint, the composition and content of which are as follows by mass:
[0237] Component A: 55 parts of water-based epoxy resin emulsion;
[0238] Component B: 55 parts of water-based epoxy resin curing agent, 24 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 6 parts of precipitated barium sulfate, 11 parts of rutile titanium dioxide, 0.4 parts of water-soluble defoaming agent, 0.2 parts of water-soluble brightening and leveling agent, 0.4 parts of water-soluble anti-sagging agent, 0.5 parts of water-soluble thickener, and 6.9 parts of water;
[0239] The specific preparation method of the ceramic microspheres with aminosilane coupling agent fixed on the surface is as follows:
[0240] A method for preparing ceramic microspheres with a particle size of 30 to 80 μm and an aminosilane coupling agent fixed on the surface:
[0241] The first step is slurry preparation
[0242] 47 parts of calcined kaolin with a particle size of 30 to 50 nm, 24 parts of spherical amorphous silicon powder with a particle size of 30 to 50 nm, and 28 parts of deionized water are added to a ball mill, and after ball milling and mixing for 30 minutes, 1.1 parts of dispersant sodium hexametaphosphate are added, and after ball milling and mixing for 1.5 hours, 1.4 parts of binder sodium carboxymethyl cellulose are added, and the mixture is ball milled and mixed for 3.5 hours to obtain a slurry;
[0243] The second step is spray drying
[0244] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 21000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0245] The third step is microsphere sintering
[0246] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0247] Step 4: Surface modification
[0248] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 2.3 parts of a first catalyst having a particle size of 30 to 50 nm. Silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0249] Step 5: Alcoholysis
[0250] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 70 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are obtained by filtration, and the reaction temperature is 60-70° C. and the reaction time is 4 hours;
[0251] Step 6: Addition reaction
[0252] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and an addition reaction is carried out with 17 parts of 3-chloropropylene in the presence of 1 to 2.5 parts of a second catalyst with a particle size of 30 to 50 nm, the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropyl alkoxysilane, and the ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0253] Step 7: Ammonolysis
[0254] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to an aminolysis reaction with 53 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate an aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with the aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0255] The method of water-based porcelain coating described in this embodiment is completed as follows:
[0256] In the first step, 55 parts of a water-based epoxy resin curing agent, 24 parts of ceramic microspheres with an aminosilane coupling agent fixed on the surface, 6 parts of precipitated barium sulfate, 11 parts of rutile titanium dioxide, 0.4 parts of a water-soluble defoaming agent, 0.2 parts of a water-soluble gloss-enhancing leveling agent, 0.4 parts of a water-soluble anti-sagging agent, 0.5 parts of a water-soluble thickener, and 6.9 parts of water are mixed uniformly to obtain component B;
[0257] In the second step, component B is mixed evenly with component A consisting of 55 parts of water-based epoxy resin emulsion to obtain a water-based porcelain coating.
[0258] Example 10
[0259] A water-based porcelain paint, the composition and content of which are as follows by mass:
[0260] Component A: 55 parts of water-based epoxy resin emulsion;
[0261] Component B: 55 parts of water-based epoxy resin curing agent, 23 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 5 parts of precipitated barium sulfate, 10 parts of rutile titanium dioxide, 0.5 parts of water-soluble defoaming agent, 0.3 parts of water-soluble brightening and leveling agent, 0.3 parts of water-soluble anti-sagging agent, 0.3 parts of water-soluble thickener, and 6.7 parts of water;
[0262] The specific preparation method of the ceramic microspheres with aminosilane coupling agent fixed on the surface is as follows:
[0263] A method for preparing ceramic microspheres with a particle size of 50 to 100 μm and an aminosilane coupling agent fixed on the surface:
[0264] The first step is slurry preparation
[0265] 46 parts of calcined kaolin with a particle size of 30-50 nm, 25 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 25 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 1.3 parts of dispersant tetramethylammonium hydroxide are added, and after ball milling and mixing for 1.5 hours, 1.5 parts of binder methyl cellulose are added, and the mixture is ball milled and mixed for another 4 hours to obtain a slurry;
[0266] The second step is spray drying
[0267] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 13000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0268] The third step is microsphere sintering
[0269] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0270] Step 4: Surface modification
[0271] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 1.6 parts of a first catalyst having a particle size of 30 to 50 nm. Silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0272] Step 5: Alcoholysis
[0273] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 45 parts of an alcoholysis agent under the protection of an inert gas, and the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, which is filtered to obtain ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface, the reaction temperature is 60-70° C., and the reaction time is 4 hours;
[0274] Step 6: Addition reaction
[0275] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and an addition reaction is carried out with 18 parts of 3-chloropropylene in the presence of 2.5 parts of a second catalyst with a particle size of 30 to 50 nm, and the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropylalkoxysilane, and the ceramic microspheres with 3-chloropropylalkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0276] Step 7: Ammonolysis
[0277] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to aminolysis reaction with 45 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0278] The method of water-based porcelain coating described in this embodiment is completed as follows:
[0279] In the first step, 55 parts of a water-based epoxy resin curing agent, 23 parts of ceramic microspheres with an aminosilane coupling agent fixed on the surface, 5 parts of precipitated barium sulfate, 10 parts of rutile titanium dioxide, 0.5 parts of a water-soluble defoaming agent, 0.3 parts of a water-soluble gloss-enhancing leveling agent, 0.3 parts of a water-soluble anti-sagging agent, 0.3 parts of a water-soluble thickener, and 6.7 parts of water are uniformly mixed to obtain component B;
[0280] In the second step, component B is mixed evenly with component A consisting of 55 parts of water-based epoxy resin emulsion to obtain a water-based porcelain coating.
[0281] Figure 1 In the figure, a is the infrared spectrum of ceramic microspheres with aminosilane coupling agent fixed on the surface, and b is the infrared spectrum of ordinary ceramic microspheres. Both a and b have obvious absorption peaks near 3400-1, 1192cm-1 and 1084cm-1. The absorption peak near 3400-1 is the stretching vibration peak of -OH, and the absorption peaks near 1192cm-1 and 1084cm-1 are the stretching vibration peaks of Si-O. In comparison, 3349cm-1 in a is the stretching vibration peak of N-H, and 2939cm-1 is the saturated carbon-hydrogen bond. The stretching vibration absorption peak of 1365cm-1 is the stretching vibration of C—N, indicating that the ceramic microspheres with aminosilane coupling agent fixed on the surface have molecular bonds of organic groups, while the peak areas of the absorption peaks near 1192cm-1 and 1084cm-1 in Figure a are significantly larger than those in Figure b, indicating that the ceramic microspheres with aminosilane coupling agent fixed on the surface have more inorganic groups, which indirectly reflects the coexistence of inorganic and organic groups in the ceramic microspheres, which proves that the present application successfully fixed the aminosilane coupling agent on the surface of the ceramic microspheres.
[0282] Table 1 Performance comparison of water-based porcelain coating of the present invention and other coatings
[0283]
[0284] Note: Comparison 1 and Comparison 2 are general porcelain coatings, and Comparison 3 is general (non-porcelain) coating.
[0285] A water-based porcelain coating of the present application has excellent performance in terms of impact resistance, water resistance, salt resistance, etc., while having a pencil hardness of 4H, while the pencil hardness of a general porcelain coating can reach 2H; the scrub resistance can reach more than 20,000 times, while the scrub resistance of a general porcelain coating is generally required to reach more than 10,000 times; and the stain resistance and stain resistance durability are also significantly improved.
[0286] In terms of stain resistance, the comprehensive stain resistance (60° gloss value) of the water-based porcelain coating of the present application is basically stable at more than 80, and it is a high-gloss coating (generally, coatings with a 60° gloss value of >60 are called high-gloss coatings), and has a good light reflection effect. The absolute value of the gloss change difference is stable at 0.7-0.8, while the absolute value of the gloss change difference of general porcelain coatings is stable at 2-3, and the absolute value of the gloss change difference of general coatings is stable at about 5, indicating that the water-based porcelain coating of the present application has good stain resistance, and pollution and scrubbing operations have little effect on the gloss of the coating surface.
[0287] In terms of stain resistance, after repeated contamination and scrubbing, the comprehensive stain resistance (60° gloss value) of the coating surface of the water-based porcelain coating of the present application decreased slightly, but it was still above 80. The absolute value of the gloss change difference increased steadily, reaching about 1, but the absolute value of the gloss change difference of general porcelain coatings was stable at 3-4, and the absolute value of the gloss change difference of general coatings reached more than 7, indicating that the water-based porcelain coating of the present application has good stain resistance and persistence, and repeated contamination and scrubbing operations have little effect on the gloss of the coating surface.
Claims
1. A water-based porcelain paint, characterized in that: Its composition and content by mass are: Component A: 47-55 parts of water-based epoxy resin emulsion; Component B: 47-55 parts of waterborne epoxy resin curing agent, 25-22 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 10-5 parts of precipitated barium sulfate, 9-11 parts of rutile titanium dioxide, 0.5-0.1 parts of defoaming agent, 0.4-0.2 parts of brightening and leveling agent, 0.4-0.2 parts of anti-sagging agent, 0.5-0.3 parts of thickener, and 7.2-6.2 parts of water; The specific preparation method of the ceramic microspheres with aminosilane coupling agent fixed on the surface is as follows: The first step is slurry preparation 45-50 parts of calcined kaolin with a particle size of 30-50 nm, 10-25 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 45-25 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 0.3-1.3 parts of a dispersant are added, and after ball milling and mixing for 1.5 hours, 0.3-1.5 parts of a binder are added, and the ball milling and mixing is continued for 2-4 hours to obtain a slurry; The second step is spray drying The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 8000-25000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min; The third step is microsphere sintering The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres; Step 4: Surface modification The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 1 to 2.5 parts of a first catalyst having a particle size of 30 to 50 nm, silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening, the reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours; Step 5: Alcoholysis The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 30 to 75 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are filtered to obtain the ceramic microspheres, the reaction temperature is 60 to 70° C., and the reaction time is 4 hours; Step 6: Addition reaction The ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and 10 to 25 parts of 3-chloropropylene are subjected to an addition reaction under the action of 1 to 2.5 parts of a second catalyst with a particle size of 30 to 50 nm, and the hydrogen-containing alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropyl alkoxysilane, and the ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours; Step 7: Ammonolysis The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor, and subjected to aminolysis reaction with 20 to 50 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate aminosilane coupling agent. The reaction temperature is 85 to 95°C. After the reaction is completed, the ceramic microspheres with aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5 hours. Step 8: Preparation of water-based porcelain paint Mix 47-55 parts of waterborne epoxy resin curing agent in component B, 25-22 parts of ceramic microspheres with aminosilane coupling agent fixed on the surface, 10-5 parts of precipitated barium sulfate, 9-11 parts of rutile titanium dioxide, 0.5-0.1 parts of defoaming agent, 0.4-0.2 parts of gloss enhancing and leveling agent, 0.4-0.2 parts of anti-sagging agent, 0.5-0.3 parts of thickener, and 7.2-6.2 parts of water evenly; Then, the evenly mixed mixture of component B is evenly mixed with 47 to 55 parts of the water-based epoxy resin emulsion of component A to obtain a water-based porcelain coating.
2. The water-based porcelain paint according to claim 1, characterized in that: The dispersant is any one of tetramethylammonium hydroxide, sodium hexametaphosphate, polyacrylate, citrate and sodium humate.
3. The water-based porcelain paint according to claim 1, characterized in that: The binder is any one of sodium cellulose, methyl cellulose, polyvinyl alcohol, polypropylene, saccharin, dextrin, starch and gum arabic.
4. The water-based porcelain paint according to claim 1, characterized in that: The first catalyst is any one of a copper-based catalyst and an iron-based catalyst.
5. The water-based porcelain paint according to claim 1, characterized in that: The alcoholysis agent is any one of methanol and ethanol.
6. The water-based porcelain paint according to claim 1, characterized in that: The second catalyst is hydrated ruthenium trichloride.
7. The water-based porcelain paint according to claim 1, characterized in that: The defoamer, gloss-enhancing and leveling agent, anti-sagging agent and thickener are all water-soluble compounds.
8. A method for preparing the water-based porcelain coating according to any one of claims 1 to 7, characterized in that: Complete it as follows: The first step is to uniformly mix 47-55 parts of a waterborne epoxy resin curing agent, 25-22 parts of ceramic microspheres with an aminosilane coupling agent fixed on the surface, 10-5 parts of precipitated barium sulfate, 9-11 parts of rutile titanium dioxide, 0.5-0.1 parts of a defoaming agent, 0.4-0.2 parts of a gloss-enhancing leveling agent, 0.4-0.2 parts of an anti-sagging agent, 0.5-0.3 parts of a thickener, and 7.2-6.2 parts of water to obtain component B; In the second step, component B is mixed evenly with component A consisting of 47 to 55 parts of water-based epoxy resin emulsion to obtain a water-based porcelain coating.
Citation Information
Patent Citations
Waterborne epoxy resin porcelain coating and preparation method thereof
CN110172289A
Environment-friendly and easy-to-clean tunnel highlight porcelainized coating and preparation method thereof
CN115960529A
Water-based high-strength porcelainized coating and preparation method thereof
CN116285617A
Modification method of ceramic powder, microwave dielectric ceramic slurry as well as preparation method and application of microwave dielectric ceramic slurry
CN117362049A
Method for circularly producing silane coupling agent
CN101519413A