Anti-corrosion powder coating with good impact resistance and preparation method thereof
By introducing elastomer composite materials and modified basalt fibers into anticorrosion powder coatings, combined with nanotitanium dioxide and ethyl orthosilicate treatment, the problem of insufficient impact resistance of traditional coatings is solved, and a high toughness and adhesion coating is achieved, which is significantly Improves impact resistance and service life and simplifies the preparation process.
Patent Information
- Application Number
- CN202411138592.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional anti-corrosion powder coatings lack impact resistance in extreme use environments, making it difficult to maintain the integrity and adhesion of the coating. Existing improvement methods often sacrifice hardness, wear resistance or increase preparation cost and process complexity, making it difficult to achieve comprehensive performance. Optimal balance.
Using specific component selection and unique preparation processes, the coating with high toughness and adhesion is formed by introducing elastomer composite materials and modified basalt fibers, combined with nanotitanium dioxide and ethyl orthosilicate, and the coating is enhanced. Impact resistance.
It significantly improves the impact resistance of the coating, maintains excellent adhesion and wear resistance, while reducing the risk of coating cracking and peeling, extends service life, and simplifies the preparation process, which is suitable for large-scale industrial production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to an anticorrosive powder coating with good impact resistance and a preparation method thereof. Background Art
[0002] In the rapidly developing automobile manufacturing, home appliance manufacturing and construction industries, powder coatings are increasingly favored due to their environmental protection, energy saving and high efficiency. In particular, anti-corrosion powder coatings, with their excellent adhesion, heat resistance, chemical resistance and wear resistance, have occupied an important position in the coating of various metal substrates. However, with the continuous improvement of industrial products' requirements for durability and impact resistance, traditional anti-corrosion powder coatings are still insufficient in certain extreme use environments, especially on parts that are susceptible to external impact, such as automobile bumpers and body exterior trims, the impact resistance of the coating has become an urgent problem to be solved.
[0003] Anti-corrosion powder coatings are mainly composed of epoxy resin, curing agent, pigment, filler and additives, and are prepared by melt mixing and extrusion. The epoxy resin has excellent adhesion to metal substrates due to its molecular structure containing a large number of benzene rings, ether bonds and hydroxyl groups, and can form a high hardness and high wear resistance coating after curing. However, the impact resistance of traditional anti-corrosion powder coatings is limited by its brittleness after curing, and it is difficult to maintain the integrity and adhesion of the coating when subjected to strong impact.
[0004] There are many methods on the market to improve the impact resistance of anti-corrosion powder coatings, such as adding elastomers and toughening agents. However, these methods often sacrifice some of the hardness, wear resistance or chemical resistance of the coating, making it difficult to achieve the optimal balance of comprehensive performance. In addition, some modification methods also increase the preparation cost and process complexity of the coating, which is not conducive to large-scale industrial production.
[0005] In view of the above problems, the present invention proposes a novel anti-corrosion powder coating with good impact resistance and a preparation method thereof. Summary of the invention
[0006] The present invention provides an anti-corrosion powder coating with good impact resistance and a preparation method thereof, aiming to achieve the coating having excellent adhesion and wear resistance while significantly improving its impact resistance through specific component selection and a unique preparation process.
[0007] The technical solution of the present invention is as follows: In the first aspect, the present invention provides an anti-corrosion powder coating with good impact resistance, which is composed of the following raw materials in parts by weight: 50-60 parts of epoxy resin, 35-45 parts of polyester resin, 10-14 parts of curing agent, 2.4-3 parts of elastomer composite material, 10-14 parts of modified basalt fiber, and 1.6-2 parts of leveling agent.
[0008] As a further technical solution, the preparation method of the elastomer composite material comprises: dissolving maleic anhydride in acetone by ultrasonication, mixing with POE and nano-titanium dioxide after complete dissolution, drying, and then melt-blending to prepare the elastomer composite material.
[0009] As a further technical solution, the dosage ratio of maleic anhydride, acetone, POE and nano-titanium dioxide is (6-7) g: (70-80) mL: (12-14) g: (560-600) g.
[0010] As a further technical solution, the raw materials of the modified basalt fiber include a modifier and basalt fiber. The components of the basalt fiber, in weight percentage, are SiO2 40.6%-41.2%, Al2O3 37.5%-37.9%, MgO 10.2%-10.4%, CaO 6.8%-7.2%, TiO2 1.2%-1.4%, Fe2O3 0.4%-0.6% and other impurities.
[0011] As a further technical solution, the average length of the basalt fiber is 62-68 μm and the diameter is 3-4 μm.
[0012] As a further technical solution, the preparation method of the modified basalt fiber includes: ultrasonically dispersing the pretreated basalt fiber in ethanol, adding tetraethyl orthosilicate at 45-55°C, and adding ammonia water to adjust the pH to 8.5-9.5, stirring at a constant temperature for 4-5 hours, and continuing to age for 10-12 hours after the reaction is completed, washing and drying to obtain nano-silicon dioxide modified basalt fiber.
[0013] As a further technical solution, the basalt fiber is pretreated by immersing the basalt fiber in a sodium hydroxide aqueous solution with a mass fraction of 5%-6% for 3.5-4.5 hours, and then filtering, washing and drying.
[0014] As a further technical solution, the usage ratio of the pretreated basalt fiber, ethanol, and ethyl orthosilicate is (14-16) g: (60-80) mL: (1-1.2) g.
[0015] As a further technical solution, the epoxy resin is bisphenol A epoxy resin model E-12.
[0016] As a further technical solution, the polyester resin is unsaturated polyester resin HR-8309C.
[0017] As a further technical solution, the curing agent is Huangshan Xinjia HB510.
[0018] As a further technical solution, the leveling agent is BYK-333 from Germany.
[0019] In a second aspect, the present invention provides a method for preparing an anticorrosive powder coating having good impact resistance, the steps comprising: (1) Preparation of elastomer composites and modified basalt fibers; (2) weighing the raw materials according to the proportion and mixing them evenly, and feeding the mixed material into a twin-screw extruder for melt extrusion, and then pressing the mixed material through a twin-roller to obtain a sheet material; (3) Crush the flake material and pass it through a 200-mesh sieve to obtain a powder coating.
[0020] As a further technical solution, the temperature of each zone of the twin-screw extruder is set as follows: zone 1 temperature 124-126°C, zone 2 temperature 120-124°C, zone 3 temperature 117-119°C, and die head temperature 120-122°C; the main engine speed of the twin-screw extruder is 121-125r / min.
[0021] The working principle and beneficial effects of the present invention are: 1. The present invention introduces elastomer composite materials and modified basalt fibers as key components, which effectively enhance the toughness and strength of the coating, so that the coating can absorb more energy and disperse stress when subjected to external impact, thereby significantly reducing the risk of cracking or peeling of the coating and significantly improving the impact resistance of the coating.
[0022] 2. The present invention ultrasonically dissolves maleic anhydride in acetone, and melt-blends after being fully mixed with POE (polyolefin elastomer) and nano-titanium dioxide. The elastomer and nano-titanium dioxide in the obtained elastomer composite material can also produce a synergistic effect, effectively enhancing the flexibility and toughness of the coating. This composite material acts as a toughening agent in the coating, which can effectively absorb and disperse energy when impacted, thereby significantly improving the impact resistance of the coating. At the same time, its unique molecular structure and good compatibility with the resin matrix also ensure the excellent adhesion between the coating and the substrate, avoiding the peeling and cracking problems of the coating during long-term use. In addition, the addition of nano-titanium dioxide not only enhances the mechanical properties of the elastomer composite material, but also gives the coating good wear resistance. This is because the nano effect of nano-titanium dioxide enables it to form uniformly distributed hard points in the coating, which can effectively resist the erosion of external friction when the coating is worn, thereby extending the service life of the coating. In addition, nano-titanium dioxide can also form a stable chemical bond with the resin matrix to improve the overall strength and wear resistance of the coating.
[0023] 3. The basalt fiber used in the present invention provides excellent mechanical reinforcement for the coating with its high strength and high modulus. In the present invention, the high strength and high modulus of the fiber itself are ensured by strictly controlling the composition of the basalt fiber. At the same time, by adjusting the average length (62-68μm) and diameter (3-4μm) of the fiber, the average length and diameter are optimized so that it can be evenly dispersed in the coating to form an effective reinforcement network, further improving the dispersion and reinforcement effect of the fiber in the coating. In particular, the basalt fiber modified with nano-silicon dioxide plays a skeleton role in the coating, which can withstand and disperse external impact and stress, thereby significantly improving the impact resistance of the coating.
[0024] 4. The present invention successfully coated a layer of nano-silicon dioxide on the surface of the fiber by ultrasonically dispersing the pretreated basalt fiber in ethanol and adding ethyl orthosilicate to react under specific temperature and pH conditions. The surface treatment of basalt fiber with nano-silicon dioxide not only maintains the high strength and high modulus characteristics of the basalt fiber itself, but also further improves the interfacial bonding force between the fiber and the resin matrix, thereby significantly improving the overall impact resistance of the coating. When the coating is subjected to external force, the nano-oxide particles can act as stress concentration points to disperse and transfer the external force to the surrounding resin matrix. This stress dispersion and transfer mechanism can reduce the stress concentration phenomenon inside the coating and prevent the coating from being damaged due to excessive local stress. At the same time, the nanoparticles can also absorb part of the energy, slow down the impact of external force on the coating, and improve the impact resistance of the coating. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1 In this embodiment, an anticorrosive powder coating with good impact resistance is provided, which is composed of the following raw materials in parts by weight: 55 parts of epoxy resin, 40 parts of polyester resin, 12 parts of curing agent, 2.7 parts of elastomer composite material, 12 parts of modified basalt fiber, and 1.8 parts of leveling agent; The preparation method of the elastomer composite material comprises: ultrasonically dissolving maleic anhydride in acetone, mixing with POE and nano-titanium dioxide after the maleic anhydride is completely dissolved, and then naturally drying and then melt blending on a co-rotating twin-screw extruder to prepare the elastomer composite material; the dosage ratio of maleic anhydride, acetone, POE and nano-titanium dioxide is 6.5g:75mL:13g:580g; The preparation method of the modified basalt fiber includes: ultrasonically dispersing the pretreated basalt fiber in ethanol, adding tetraethyl orthosilicate at 50°C, and dropping ammonia water to adjust the pH to 9, stirring at a constant temperature for 4.5 hours, and continuing to age for 11 hours after the reaction is completed, washing and drying to obtain nano-silicon dioxide modified basalt fiber; the amount ratio of the pretreated basalt fiber, ethanol, and tetraethyl orthosilicate is 15g:70mL:1.1g; Basalt fiber pretreatment: immerse the basalt fiber in a sodium hydroxide aqueous solution with a mass fraction of 5.5% for 4 hours, and then filter, wash and dry to obtain the basalt fiber; the composition of the basalt fiber is SiO240.9%, Al2O337.7%, MgO10.3%, CaO7.0%, TiO21.3%, Fe2O30.5% and other impurities in weight percentage; the average length of the basalt fiber is 65μm and the diameter is 3.5μm; Among them, the epoxy resin is bisphenol A epoxy resin model E-12; the polyester resin is unsaturated polyester resin HR-8309C; the curing agent is Huangshan Xinjia HB510; the leveling agent is German BYK-333; and the POE is DF710 produced by Singapore Mitsui Chemicals.
[0027] The method for preparing the anticorrosive powder coating with good impact resistance comprises the following steps: (1) Preparation of elastomer composites and modified basalt fibers; (2) Weigh the raw materials according to the proportion and mix them evenly, and send the mixed materials into a twin-screw extruder for melt extrusion, and obtain a mixed material through double-roll sheeting; the temperature of each zone of the twin-screw extruder is set as follows: the temperature of zone 1 is 125°C, the temperature of zone 2 is 122°C, the temperature of zone 3 is 118°C, and the temperature of the die head is 121°C; the main engine speed of the twin-screw extruder is 123r / min; (3) The cooled flake material is crushed at high speed and then passed through a 200-mesh sieve to obtain a powder coating.
[0028] Example 2 In this embodiment, an anticorrosive powder coating with good impact resistance is provided, which is composed of the following raw materials in parts by weight: 50 parts of epoxy resin, 35 parts of polyester resin, 10 parts of curing agent, 2.4 parts of elastomer composite material, 10 parts of modified basalt fiber, and 1.6 parts of leveling agent; The preparation method of the elastomer composite material comprises: dissolving maleic anhydride in acetone by ultrasonic method, mixing with POE and nano-titanium dioxide after the maleic anhydride is completely dissolved, and then naturally drying and then melt blending on a co-rotating twin-screw extruder to prepare the elastomer composite material; the dosage ratio of maleic anhydride, acetone, POE and nano-titanium dioxide is 6g:70mL:12g:560g; The preparation method of the modified basalt fiber includes: ultrasonically dispersing the pretreated basalt fiber in ethanol, adding tetraethyl orthosilicate at 45°C, and dropping ammonia water to adjust the pH to 8.5, stirring at a constant temperature for 4 hours, and continuing to age for 10 hours after the reaction is completed, washing and drying to obtain nano-silicon dioxide modified basalt fiber; the amount ratio of the pretreated basalt fiber, ethanol, and tetraethyl orthosilicate is 14g:60mL:1g; Basalt fiber pretreatment: immerse the basalt fiber in a 5% sodium hydroxide aqueous solution for 3.5 hours, filter, wash and dry the basalt fiber; the composition of the basalt fiber is SiO240.6%, Al2O337.5%, MgO10.2%, CaO6.8%, TiO21.2%, Fe2O30.4% and other impurities in weight percentage; the average length of the basalt fiber is 62μm and the diameter is 3μm; Among them, the epoxy resin is bisphenol A epoxy resin model E-12; the polyester resin is unsaturated polyester resin HR-8309C; the curing agent is Huangshan Xinjia HB510; the leveling agent is German BYK-333; and the POE is DF710 produced by Singapore Mitsui Chemicals.
[0029] The method for preparing the anticorrosive powder coating with good impact resistance comprises the following steps: (1) Preparation of elastomer composites and modified basalt fibers; (2) Weigh the raw materials according to the proportion and mix them evenly, and send the mixed materials into a twin-screw extruder for melt extrusion, and obtain a mixed material through double-roll sheeting; the temperature of each zone of the twin-screw extruder is set as follows: the temperature of zone 1 is 124°C, the temperature of zone 2 is 120°C, the temperature of zone 3 is 117°C, and the temperature of the die head is 120°C; the main engine speed of the twin-screw extruder is 121r / min; (3) The cooled flake material is crushed at high speed and then passed through a 200-mesh sieve to obtain a powder coating.
[0030] Example 3 In this embodiment, an anticorrosive powder coating with good impact resistance is provided, which is composed of the following raw materials in parts by weight: 60 parts of epoxy resin, 45 parts of polyester resin, 14 parts of curing agent, 3 parts of elastomer composite material, 14 parts of modified basalt fiber, and 2 parts of leveling agent; The preparation method of the elastomer composite material comprises: ultrasonically dissolving maleic anhydride in acetone, mixing with POE and nano-titanium dioxide after the maleic anhydride is completely dissolved, and then naturally drying and then melt blending on a co-rotating twin-screw extruder to prepare the elastomer composite material; the dosage ratio of maleic anhydride, acetone, POE and nano-titanium dioxide is 7g:80mL:14g:600g; The preparation method of the modified basalt fiber includes: ultrasonically dispersing the pretreated basalt fiber in ethanol, adding tetraethyl orthosilicate at 55°C, and dropping ammonia water to adjust the pH to 9.5, stirring at a constant temperature for 5 hours, and continuing to age for 12 hours after the reaction is completed, washing and drying to obtain nano-silicon dioxide modified basalt fiber; the amount ratio of the pretreated basalt fiber, ethanol, and tetraethyl orthosilicate is 16g:80mL:1.2g; Basalt fiber pretreatment: immerse the basalt fiber in a sodium hydroxide aqueous solution with a mass fraction of 6% for 4.5 hours, and then filter, wash and dry to obtain the basalt fiber; the composition of the basalt fiber is SiO241.2%, Al2O337.9%, MgO10.4%, CaO7.2%, TiO21.4%, Fe2O30.6% and other impurities in weight percentage; the average length of the basalt fiber is 68μm and the diameter is 4μm; Among them, the epoxy resin is bisphenol A epoxy resin model E-12; the polyester resin is unsaturated polyester resin HR-8309C; the curing agent is Huangshan Xinjia HB510; the leveling agent is German BYK-333; and the POE is DF710 produced by Singapore Mitsui Chemicals.
[0031] The method for preparing the anticorrosive powder coating with good impact resistance comprises the following steps: (1) Preparation of elastomer composites and modified basalt fibers; (2) Weigh the raw materials according to the proportion and mix them evenly, and send the mixed materials into a twin-screw extruder for melt extrusion, and obtain a mixed material through double-roll sheeting; the temperature of each zone of the twin-screw extruder is set as follows: the temperature of zone 1 is 126°C, the temperature of zone 2 is 124°C, the temperature of zone 3 is 119°C, and the temperature of the die head is 122°C; the main engine speed of the twin-screw extruder is 125r / min; (3) The cooled flake material is crushed at high speed and then passed through a 200-mesh sieve to obtain a powder coating.
[0032] Example 4 In this embodiment, an anticorrosive powder coating with good impact resistance is provided, which is composed of the following raw materials in parts by weight: 50 parts of epoxy resin, 45 parts of polyester resin, 10 parts of curing agent, 3 parts of elastomer composite material, 10 parts of modified basalt fiber, and 2 parts of leveling agent; The preparation method of the elastomer composite material comprises: ultrasonically dissolving maleic anhydride in acetone, mixing with POE and nano-titanium dioxide after the maleic anhydride is completely dissolved, and then naturally drying and then melt blending on a co-rotating twin-screw extruder to prepare the elastomer composite material; the dosage ratio of maleic anhydride, acetone, POE and nano-titanium dioxide is 6g:80mL:12g:600g; The preparation method of the modified basalt fiber includes: ultrasonically dispersing the pretreated basalt fiber in ethanol, adding tetraethyl orthosilicate at 45°C, and dropping ammonia water to adjust the pH to 9.5, stirring at a constant temperature for 4 hours, and continuing to age for 12 hours after the reaction is completed, washing and drying to obtain nano-silicon dioxide modified basalt fiber; the amount ratio of the pretreated basalt fiber, ethanol, and tetraethyl orthosilicate is 14g:80mL:1g; Basalt fiber pretreatment: immerse the basalt fiber in a 5% sodium hydroxide aqueous solution for 4.5 hours, filter, wash and dry the basalt fiber; the composition of the basalt fiber is SiO240.6%, Al2O337.9%, MgO10.2%, CaO7.2%, TiO21.2%, Fe2O30.6% and other impurities in weight percentage; the average length of the basalt fiber is 62μm and the diameter is 4μm; Among them, the epoxy resin is bisphenol A epoxy resin model E-12; the polyester resin is unsaturated polyester resin HR-8309C; the curing agent is Huangshan Xinjia HB510; the leveling agent is German BYK-333; and the POE is DF710 produced by Singapore Mitsui Chemicals.
[0033] The method for preparing the anticorrosive powder coating with good impact resistance comprises the following steps: (1) Preparation of elastomer composites and modified basalt fibers; (2) Weigh the raw materials according to the proportion and mix them evenly, and send the mixed materials into a twin-screw extruder for melt extrusion, and obtain a mixed material through double-roll sheeting; the temperature of each zone of the twin-screw extruder is set as follows: the temperature of zone 1 is 126°C, the temperature of zone 2 is 120°C, the temperature of zone 3 is 119°C, and the temperature of the die head is 120°C; the main engine speed of the twin-screw extruder is 125r / min; (3) The cooled flake material is crushed at high speed and then passed through a 200-mesh sieve to obtain a powder coating.
[0034] Comparative Example 1 In this comparative example, an anticorrosive powder coating with good impact resistance is provided, which is composed of the following raw materials in parts by weight: 55 parts of epoxy resin, 40 parts of polyester resin, 12 parts of curing agent, 2.7 parts of elastomer composite material, 12 parts of modified basalt fiber, and 1.8 parts of leveling agent; The preparation method of the elastomer composite material includes: ultrasonically dissolving maleic anhydride in acetone, mixing with POE after complete dissolution, and then naturally drying and melt blending on a co-rotating twin-screw extruder to prepare the elastomer composite material; the amount ratio of maleic anhydride, acetone and POE is 6.5g:75mL:13g; The preparation method of the modified basalt fiber includes: ultrasonically dispersing the pretreated basalt fiber in ethanol, adding tetraethyl orthosilicate at 50°C, and dropping ammonia water to adjust the pH to 9, stirring at a constant temperature for 4.5 hours, and continuing to age for 11 hours after the reaction is completed, washing and drying to obtain nano-silicon dioxide modified basalt fiber; the amount ratio of the pretreated basalt fiber, ethanol, and tetraethyl orthosilicate is 15g:70mL:1.1g; Basalt fiber pretreatment: immerse the basalt fiber in a sodium hydroxide aqueous solution with a mass fraction of 5.5% for 4 hours, and then filter, wash and dry to obtain the basalt fiber; the composition of the basalt fiber is SiO240.9%, Al2O337.7%, MgO10.3%, CaO7.0%, TiO21.3%, Fe2O30.5% and other impurities in weight percentage; the average length of the basalt fiber is 65μm and the diameter is 3.5μm; Among them, the epoxy resin is bisphenol A epoxy resin model E-12; the polyester resin is unsaturated polyester resin HR-8309C; the curing agent is Huangshan Xinjia HB510; the leveling agent is German BYK-333; and the POE is DF710 produced by Singapore Mitsui Chemicals.
[0035] The method for preparing the anticorrosive powder coating with good impact resistance comprises the following steps: (1) Preparation of elastomer composites and modified basalt fibers; (2) Weigh the raw materials according to the proportion and mix them evenly, and send the mixed materials into a twin-screw extruder for melt extrusion, and obtain a mixed material through double-roll sheeting; the temperature of each zone of the twin-screw extruder is set as follows: the temperature of zone 1 is 125°C, the temperature of zone 2 is 122°C, the temperature of zone 3 is 118°C, and the temperature of the die head is 121°C; the main engine speed of the twin-screw extruder is 123r / min; (3) The cooled flake material is crushed at high speed and then passed through a 200-mesh sieve to obtain a powder coating.
[0036] Comparative Example 2 In this comparative example, an anticorrosive powder coating with good impact resistance is provided, which is composed of the following raw materials in parts by weight: 55 parts of epoxy resin, 40 parts of polyester resin, 12 parts of curing agent, 2.7 parts of elastomer composite material, 12 parts of modified basalt fiber, and 1.8 parts of leveling agent; The preparation method of the elastomer composite material comprises: ultrasonically dissolving maleic anhydride in acetone, mixing with POE and nano-silicon dioxide after the maleic anhydride is completely dissolved, and then naturally drying and then melt blending on a co-rotating twin-screw extruder to prepare the elastomer composite material; the dosage ratio of maleic anhydride, acetone, POE and nano-silicon dioxide is 6.5g:75mL:13g:580g; The preparation method of the modified basalt fiber includes: ultrasonically dispersing the pretreated basalt fiber in ethanol, adding tetraethyl orthosilicate at 50°C, and dropping ammonia water to adjust the pH to 9, stirring at a constant temperature for 4.5 hours, and continuing to age for 11 hours after the reaction is completed, washing and drying to obtain nano-silicon dioxide modified basalt fiber; the amount ratio of the pretreated basalt fiber, ethanol, and tetraethyl orthosilicate is 15g:70mL:1.1g; Basalt fiber pretreatment: immerse the basalt fiber in a sodium hydroxide aqueous solution with a mass fraction of 5.5% for 4 hours, and then filter, wash and dry to obtain the basalt fiber; the composition of the basalt fiber is SiO240.9%, Al2O337.7%, MgO10.3%, CaO7.0%, TiO21.3%, Fe2O30.5% and other impurities in weight percentage; the average length of the basalt fiber is 65μm and the diameter is 3.5μm; Among them, the epoxy resin is bisphenol A epoxy resin model E-12; the polyester resin is unsaturated polyester resin HR-8309C; the curing agent is Huangshan Xinjia HB510; the leveling agent is German BYK-333; and the POE is DF710 produced by Singapore Mitsui Chemicals.
[0037] The method for preparing the anticorrosive powder coating with good impact resistance comprises the following steps: (1) Preparation of elastomer composites and modified basalt fibers; (2) Weigh the raw materials according to the proportion and mix them evenly, and send the mixed materials into a twin-screw extruder for melt extrusion, and obtain a mixed material through double-roll sheeting; the temperature of each zone of the twin-screw extruder is set as follows: the temperature of zone 1 is 125°C, the temperature of zone 2 is 122°C, the temperature of zone 3 is 118°C, and the temperature of the die head is 121°C; the main engine speed of the twin-screw extruder is 123r / min; (3) The cooled flake material is crushed at high speed and then passed through a 200-mesh sieve to obtain a powder coating.
[0038] Comparative Example 3 In this comparative example, an anticorrosive powder coating with good impact resistance is provided, which is composed of the following raw materials in parts by weight: 55 parts of epoxy resin, 40 parts of polyester resin, 12 parts of curing agent, 2.7 parts of elastomer composite material, 12 parts of modified basalt fiber, and 1.8 parts of leveling agent; The preparation method of the elastomer composite material comprises: ultrasonically dissolving maleic anhydride in acetone, mixing with POE and nano-titanium dioxide after the maleic anhydride is completely dissolved, and then naturally drying and then melt blending on a co-rotating twin-screw extruder to prepare the elastomer composite material; the dosage ratio of maleic anhydride, acetone, POE and nano-titanium dioxide is 6.5g:75mL:13g:580g; The preparation method of modified basalt fiber includes: ultrasonically dispersing basalt fiber in ethanol, adding tetraethyl orthosilicate at 50°C, and dropping ammonia water to adjust the pH to 9, stirring at a constant temperature for 4.5 hours, and continuing to age for 11 hours after the reaction is completed, washing and drying to obtain nano-silicon dioxide modified basalt fiber; the dosage ratio of basalt fiber, ethanol, and tetraethyl orthosilicate is 15g:70mL:1.1g; the composition of basalt fiber is SiO240.9%, Al2O337.7%, MgO10.3%, CaO7.0%, TiO21.3%, Fe2O30.5% and other impurities in weight percentage; the average length of basalt fiber is 65μm and the diameter is 3.5μm; Among them, the epoxy resin is bisphenol A epoxy resin model E-12; the polyester resin is unsaturated polyester resin HR-8309C; the curing agent is Huangshan Xinjia HB510; the leveling agent is German BYK-333; and the POE is DF710 produced by Singapore Mitsui Chemicals.
[0039] The method for preparing the anticorrosive powder coating with good impact resistance comprises the following steps: (1) Preparation of elastomer composites and modified basalt fibers; (2) Weigh the raw materials according to the proportion and mix them evenly, and send the mixed materials into a twin-screw extruder for melt extrusion, and obtain a mixed material through double-roll sheeting; the temperature of each zone of the twin-screw extruder is set as follows: the temperature of zone 1 is 125°C, the temperature of zone 2 is 122°C, the temperature of zone 3 is 118°C, and the temperature of the die head is 121°C; the main engine speed of the twin-screw extruder is 123r / min; (3) The cooled flake material is crushed at high speed and then passed through a 200-mesh sieve to obtain a powder coating.
[0040] Comparative Example 4 In this comparative example, an anticorrosive powder coating with good impact resistance is provided, which is composed of the following raw materials in parts by weight: 55 parts of epoxy resin, 40 parts of polyester resin, 12 parts of curing agent, 2.7 parts of elastomer composite material, 12 parts of basalt fiber, and 1.8 parts of leveling agent; The preparation method of the elastomer composite material comprises: ultrasonically dissolving maleic anhydride in acetone, mixing with POE and nano-titanium dioxide after the maleic anhydride is completely dissolved, and then naturally drying and then melt blending on a co-rotating twin-screw extruder to prepare the elastomer composite material; the dosage ratio of maleic anhydride, acetone, POE and nano-titanium dioxide is 6.5g:75mL:13g:580g; The basalt fiber is a pre-treated basalt fiber: the basalt fiber is immersed in a sodium hydroxide aqueous solution with a mass fraction of 5.5% for 4 hours, and then filtered, washed and dried; the composition of the basalt fiber is SiO240.9%, Al2O337.7%, MgO10.3%, CaO7.0%, TiO21.3%, Fe2O30.5% and other impurities in weight percentage; the average length of the basalt fiber is 65μm and the diameter is 3.5μm; Among them, the epoxy resin is bisphenol A epoxy resin model E-12; the polyester resin is unsaturated polyester resin HR-8309C; the curing agent is Huangshan Xinjia HB510; the leveling agent is German BYK-333; and the POE is DF710 produced by Singapore Mitsui Chemicals.
[0041] The method for preparing the anticorrosive powder coating with good impact resistance comprises the following steps: (1) Preparation of elastomer composites and modified basalt fibers; (2) Weigh the raw materials according to the proportion and mix them evenly, and send the mixed materials into a twin-screw extruder for melt extrusion, and obtain a mixed material through double-roll sheeting; the temperature of each zone of the twin-screw extruder is set as follows: the temperature of zone 1 is 125°C, the temperature of zone 2 is 122°C, the temperature of zone 3 is 118°C, and the temperature of the die head is 121°C; the main engine speed of the twin-screw extruder is 123r / min; (3) The cooled flake material is crushed at high speed and then passed through a 200-mesh sieve to obtain a powder coating.
[0042] Comparative Example 5 In this comparative example, an anticorrosive powder coating with good impact resistance is provided, which is composed of the following raw materials in parts by weight: 55 parts of epoxy resin, 40 parts of polyester resin, 12 parts of curing agent, 2.7 parts of elastomer composite material, 12 parts of basalt fiber, and 1.8 parts of leveling agent; The preparation method of the elastomer composite material comprises: ultrasonically dissolving maleic anhydride in acetone, mixing with POE and nano-titanium dioxide after the maleic anhydride is completely dissolved, and then naturally drying and then melt blending on a co-rotating twin-screw extruder to prepare the elastomer composite material; the dosage ratio of maleic anhydride, acetone, POE and nano-titanium dioxide is 6.5g:75mL:13g:580g; The composition of basalt fiber is SiO240.9%, Al2O337.7%, MgO10.3%, CaO7.0%, TiO21.3%, Fe2O30.5% and other impurities in terms of weight percentage; the average length of basalt fiber is 65μm and the diameter is 3.5μm; Among them, the epoxy resin is bisphenol A epoxy resin model E-12; the polyester resin is unsaturated polyester resin HR-8309C; the curing agent is Huangshan Xinjia HB510; the leveling agent is German BYK-333; and the POE is DF710 produced by Singapore Mitsui Chemicals.
[0043] The method for preparing the anticorrosive powder coating with good impact resistance comprises the following steps: (1) Preparation of elastomer composites and modified basalt fibers; (2) Weigh the raw materials according to the proportion and mix them evenly, and send the mixed materials into a twin-screw extruder for melt extrusion, and obtain a mixed material through double-roll sheeting; the temperature of each zone of the twin-screw extruder is set as follows: the temperature of zone 1 is 125°C, the temperature of zone 2 is 122°C, the temperature of zone 3 is 118°C, and the temperature of the die head is 121°C; the main engine speed of the twin-screw extruder is 123r / min; (3) The cooled flake material is crushed at high speed and then passed through a 200-mesh sieve to obtain a powder coating.
[0044] Comparative Example 6 In this comparative example, an anticorrosive powder coating with good impact resistance is provided, which is composed of the following raw materials in parts by weight: 55 parts of epoxy resin, 40 parts of polyester resin, 12 parts of curing agent, 2.7 parts of elastomer composite material, 12 parts of modified basalt fiber, and 1.8 parts of leveling agent; The preparation method of the elastomer composite material comprises: ultrasonically dissolving maleic anhydride in acetone, mixing with POE and nano-titanium dioxide after the maleic anhydride is completely dissolved, and then naturally drying and then melt blending on a co-rotating twin-screw extruder to prepare the elastomer composite material; the dosage ratio of maleic anhydride, acetone, POE and nano-titanium dioxide is 6.5g:75mL:13g:580g; The preparation method of the modified basalt fiber includes: ultrasonically dispersing the pretreated basalt fiber in ethanol, adding tetraethyl orthosilicate at 50°C, and dropping ammonia water to adjust the pH to 9, stirring at a constant temperature for 4.5 hours, and continuing to age for 11 hours after the reaction is completed, washing and drying to obtain nano-silicon dioxide modified basalt fiber; the amount ratio of the pretreated basalt fiber, ethanol, and tetraethyl orthosilicate is 15g:70mL:1.1g; Basalt fiber pretreatment: immerse the basalt fiber in a sodium hydroxide aqueous solution with a mass fraction of 5.5% for 4 hours, and then filter, wash and dry to obtain the basalt fiber; the composition of the basalt fiber is SiO245.9%, Al2O330.7%, MgO8.3%, CaO8.0%, TiO22.3%, Fe2O31.5% and other impurities in weight percentage; the average length of the basalt fiber is 65μm and the diameter is 3.5μm; Among them, the epoxy resin is bisphenol A epoxy resin model E-12; the polyester resin is unsaturated polyester resin HR-8309C; the curing agent is Huangshan Xinjia HB510; the leveling agent is German BYK-333; and the POE is DF710 produced by Singapore Mitsui Chemicals.
[0045] The method for preparing the anticorrosive powder coating with good impact resistance comprises the following steps: (1) Preparation of elastomer composites and modified basalt fibers; (2) Weigh the raw materials according to the proportion and mix them evenly, and send the mixed materials into a twin-screw extruder for melt extrusion, and obtain a mixed material through double-roll sheeting; the temperature of each zone of the twin-screw extruder is set as follows: the temperature of zone 1 is 125°C, the temperature of zone 2 is 122°C, the temperature of zone 3 is 118°C, and the temperature of the die head is 121°C; the main engine speed of the twin-screw extruder is 123r / min; (3) The cooled flake material is crushed at high speed and then passed through a 200-mesh sieve to obtain a powder coating.
[0046] Comparative Example 7 In this comparative example, an anticorrosive powder coating with good impact resistance is provided, which is composed of the following raw materials in parts by weight: 55 parts of epoxy resin, 40 parts of polyester resin, 12 parts of curing agent, 2.7 parts of elastomer composite material, 12 parts of modified basalt fiber, and 1.8 parts of leveling agent; The preparation method of the elastomer composite material comprises: ultrasonically dissolving maleic anhydride in acetone, mixing with POE and nano-titanium dioxide after the maleic anhydride is completely dissolved, and then naturally drying and then melt blending on a co-rotating twin-screw extruder to prepare the elastomer composite material; the dosage ratio of maleic anhydride, acetone, POE and nano-titanium dioxide is 6.5g:75mL:13g:580g; The preparation method of the modified basalt fiber includes: ultrasonically dispersing the pretreated basalt fiber in ethanol, adding tetraethyl orthosilicate at 50°C, and dropping ammonia water to adjust the pH to 9, stirring at a constant temperature for 4.5 hours, and continuing to age for 11 hours after the reaction is completed, washing and drying to obtain nano-silicon dioxide modified basalt fiber; the amount ratio of the pretreated basalt fiber, ethanol, and tetraethyl orthosilicate is 15g:70mL:1.1g; Basalt fiber pretreatment: immerse the basalt fiber in a sodium hydroxide aqueous solution with a mass fraction of 5.5% for 4 hours, and then filter, wash and dry to obtain the basalt fiber; the composition of the basalt fiber is SiO240.9%, Al2O337.7%, MgO10.3%, CaO7.0%, TiO21.3%, Fe2O30.5% and other impurities in weight percentage; the average length of the basalt fiber is 75μm and the diameter is 4.5μm; Among them, the epoxy resin is bisphenol A epoxy resin model E-12; the polyester resin is unsaturated polyester resin HR-8309C; the curing agent is Huangshan Xinjia HB510; the leveling agent is German BYK-333; and the POE is DF710 produced by Singapore Mitsui Chemicals.
[0047] The method for preparing the anticorrosive powder coating with good impact resistance comprises the following steps: (1) Preparation of elastomer composites and modified basalt fibers; (2) Weigh the raw materials according to the proportion and mix them evenly, and send the mixed materials into a twin-screw extruder for melt extrusion, and obtain a mixed material through double-roll sheeting; the temperature of each zone of the twin-screw extruder is set as follows: the temperature of zone 1 is 125°C, the temperature of zone 2 is 122°C, the temperature of zone 3 is 118°C, and the temperature of the die head is 121°C; the main engine speed of the twin-screw extruder is 123r / min; (3) The cooled flake material is crushed at high speed and then passed through a 200-mesh sieve to obtain a powder coating.
[0048] Comparative Example 8 In this comparative example, an anticorrosive powder coating with good impact resistance is provided, which is composed of the following raw materials in parts by weight: 55 parts of epoxy resin, 40 parts of polyester resin, 12 parts of curing agent, 2.7 parts of elastomer composite material, 12 parts of modified basalt fiber, and 1.8 parts of leveling agent; The preparation method of the elastomer composite material comprises: ultrasonically dissolving maleic anhydride in acetone, mixing with POE and nano-titanium dioxide after the maleic anhydride is completely dissolved, and then naturally drying and then melt blending on a co-rotating twin-screw extruder to prepare the elastomer composite material; the dosage ratio of maleic anhydride, acetone, POE and nano-titanium dioxide is 6.5g:75mL:13g:580g; The preparation method of the modified basalt fiber includes: ultrasonically dispersing the pretreated basalt fiber in ethanol, adding tetraethyl orthosilicate at 50°C, and dropping ammonia water to adjust the pH to 9, stirring at a constant temperature for 4.5 hours, and continuing to age for 11 hours after the reaction is completed, washing and drying to obtain nano-silicon dioxide modified basalt fiber; the amount ratio of the pretreated basalt fiber, ethanol, and tetraethyl orthosilicate is 15g:70mL:1.1g; Basalt fiber pretreatment: immerse the basalt fiber in a sodium hydroxide aqueous solution with a mass fraction of 5.5% for 4 hours, and then filter, wash and dry to obtain the basalt fiber; the composition of the basalt fiber is SiO240.9%, Al2O337.7%, MgO10.3%, CaO7.0%, TiO21.3%, Fe2O30.5% and other impurities in weight percentage; the average length of the basalt fiber is 55μm and the diameter is 2.5μm; Among them, the epoxy resin is bisphenol A epoxy resin model E-12; the polyester resin is unsaturated polyester resin HR-8309C; the curing agent is Huangshan Xinjia HB510; the leveling agent is German BYK-333; and the POE is DF710 produced by Singapore Mitsui Chemicals.
[0049] The method for preparing the anticorrosive powder coating with good impact resistance comprises the following steps: (1) Preparation of elastomer composites and modified basalt fibers; (2) Weigh the raw materials according to the proportion and mix them evenly, and send the mixed materials into a twin-screw extruder for melt extrusion, and obtain a mixed material through double-roll sheeting; the temperature of each zone of the twin-screw extruder is set as follows: the temperature of zone 1 is 125°C, the temperature of zone 2 is 122°C, the temperature of zone 3 is 118°C, and the temperature of the die head is 121°C; the main engine speed of the twin-screw extruder is 123r / min; (3) The cooled flake material is crushed at high speed and then passed through a 200-mesh sieve to obtain a powder coating.
[0050] Test Example 1: The powder coatings prepared in the above-mentioned Examples 1-4 and Comparative Examples 1-8 were sprayed on 50 mm × 100 mm aluminum sheets by high-voltage electrostatic spraying, with a coating thickness of 80 μm, a curing temperature of 200° C., and a curing time of 60 min to obtain test samples, and the performance was explored. The prepared powder coatings were tested as follows: 1. Use a paint film impactor to test the impact resistance of the coating in accordance with GB / T 1732-2020; perform three parallel tests and take the average value; 2. Wear resistance test: GB / T 23988-2009 "Falling sand method for determination of wear resistance of coatings" was used, and the test was conducted three times in parallel to obtain the average value. The larger the test value, the more falling sand is required for unit coating wear, indicating that the wear resistance of the coating is better; 3. Adhesion test: It is carried out in accordance with GB / T 9286-2021 "Scratch test for paint and varnish films". The smaller the number, the better the adhesion.
[0051] The test results are shown in Table 1 below: Table 1
[0052] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An anti-corrosion powder coating with good impact resistance, It is characterized in that The invention is composed of the following raw materials in parts by weight: 50-60 parts of epoxy resin, 35-45 parts of polyester resin, 10-14 parts of curing agent, 2.4-3 parts of elastomer composite material, 10-14 parts of modified basalt fiber and 1.6-2 parts of leveling agent.
2. The anti-corrosion powder coating having good impact resistance according to claim 1, It is characterized in that The preparation method of the elastomer composite material comprises: dissolving maleic anhydride in acetone by ultrasonication, mixing with POE and nano-titanium dioxide after the maleic anhydride is completely dissolved, drying, and then melt-blending to prepare the elastomer composite material.
3. The anti-corrosion powder coating with good impact resistance according to claim 2, It is characterized in that The dosage ratio of maleic anhydride, acetone, POE and nano-titanium dioxide is (6-7) g: (70-80) mL: (12-14) g: (560-600) g.
4. The anticorrosive powder coating having good impact resistance according to claim 1, It is characterized in that The raw materials of the modified basalt fiber include a modifier and basalt fiber. The composition of the basalt fiber is SiO 2 40.6-41.2%, Al 2 O 3 37.5-37.9%, MgO10.2-10.4%, CaO6.8-7.2%, TiO 2 1.2-1.4%, Fe 2 O 3 0.4-0.6% and other impurities.
5. The anti-corrosion powder coating with good impact resistance according to claim 4, It is characterized in that The basalt fibers have an average length of 62-68 μm and a diameter of 3-4 μm.
6. The anticorrosive powder coating having good impact resistance according to claim 1, It is characterized in that The preparation method of the modified basalt fiber comprises: ultrasonically dispersing the pretreated basalt fiber in ethanol, adding tetraethyl orthosilicate at 45-55° C., dripping ammonia water to adjust the pH value to 8.5-9.5, stirring at a constant temperature for 4-5 hours, continuing aging for 10-12 hours after the reaction is completed, washing and drying to obtain nano-silicon dioxide modified basalt fiber.
7. The anti-corrosion powder coating with good impact resistance according to claim 6, It is characterized in that The basalt fiber is pretreated in a sodium hydroxide aqueous solution with a mass fraction of 5%-6% for 3.5-4.5 hours, and then filtered, washed and dried to obtain the basalt fiber.
8. The anti-corrosion powder coating with good impact resistance according to claim 6, It is characterized in that The usage ratio of the pretreated basalt fiber, ethanol and ethyl orthosilicate is (14-16) g: (60-80) mL: (1-1.2) g.
9. A method for preparing an anticorrosive powder coating having good impact resistance as claimed in any one of claims 1 to 8, It is characterized in that the steps include: (1) Preparation of elastomer composites and modified basalt fibers; (2) weighing the raw materials according to the proportion and mixing them evenly, and feeding the mixed material into a twin-screw extruder for melt extrusion, and then pressing the mixed material through a twin-roller to obtain a sheet material; (3) Crush the flake material and pass it through a 200-mesh sieve to obtain a powder coating.
10. The method for preparing the anticorrosive powder coating with good impact resistance according to claim 9, It is characterized in that The temperature of each zone of the twin-screw extruder is set as follows: the temperature of zone 1 is 124-126°C, the temperature of zone 2 is 120-124°C, the temperature of zone 3 is 117-119°C, and the temperature of the die head is 120-122°C; the main engine speed of the twin-screw extruder is 121-125r / min.