Antirust agent for surface treatment of I-shaped iron as well as preparation method and application of antirust agent
By forming a three-layer coating structure of hydrophobic-hydrophilic-hydrophobic on the surface of I-beams, and utilizing modified graphene oxide and modified adsorbents, the problem of rust on I-beams was solved, achieving a good rust prevention effect.
Patent Information
- Application Number
- CN202411221926.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-02
AI Technical Summary
I-beams are susceptible to corrosion due to environmental factors in electromagnets, which affects their performance.
The coating adopts a three-layer coating structure consisting of hydrophobic and hydrophilic coatings. The hydrophobic coating is mainly composed of epoxy resin, combined with modified graphene oxide and modified adsorbent to form a hydrophobic-hydrophilic-hydrophobic coating structure. It forms a rust inhibitor through multiple sprayings.
It effectively reduces the contact between I-beams and water molecules, improves rust prevention, and reduces corrosion.
Smart Images

Figure BDA0005023285840000091 
Figure BDA0005023285840000101
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of rust inhibitors, and more specifically, to a rust inhibitor for surface treatment of I-beams and a preparation method and application thereof. Background Art
[0002] A jacquard machine is a textile machine used to weave textiles with complex patterns. It controls the movement of each needle through a series of punched cards or an electronic control program to weave a predetermined pattern or pattern on the fabric. Traditional jacquard machines use mechanical devices and punched cards, while modern electronic jacquard machines use electronic technology to achieve a more efficient and precise weaving process. Jacquard machines are widely used in the production of various textiles, including bedding, curtains, decorative fabrics, etc.
[0003] Electromagnet is a key component of electronic jacquard machine. Its main function in jacquard machine is to realize fast mechanical motion control. Through the attraction and release of electromagnet, the related parts of jacquard machine, such as needles and shuttles, can be controlled to move precisely according to the predetermined pattern, so as to realize complex pattern weaving. It is one of the key parts of jacquard machine that can weave complex patterns with high precision. The I-shaped iron parts in electromagnet, referred to as I-beam, are made of pure iron. After a long period of use, they are easily affected by the environment and rusted, which affects the use of electromagnet. Summary of the invention
[0004] In order to improve the anti-rust effect of I-beams, the present application provides a rust inhibitor for surface treatment of I-beams, and a preparation method and application thereof.
[0005] In the first aspect, the present application provides a rust preventive for surface treatment of I-beams, which adopts the following technical solution: A rust preventive for surface treatment of an I-beam, comprising a hydrophobic coating and a hydrophilic coating, wherein the hydrophobic coating comprises 60-70 parts of an epoxy resin, 25-30 parts of a curing agent, 10-15 parts of a filler, 1.5-2.5 parts of a dispersant, 0.2-0.6 parts of a defoamer, 1-1.5 parts of a rheological agent, 0.8-1.6 parts of a surfactant, 1-2.8 parts of modified graphene oxide and 20-35 parts of water; The hydrophilic coating comprises 40-50 parts of hydrophilic modified epoxy resin emulsion, 15-20 parts of curing agent, 8-12 parts of filler, 1.5-3 parts of dispersant, 0.1-0.4 parts of defoamer, 0.5-1 parts of rheological agent, 0.5-1 parts of surfactant and 0.2-0.5 parts of modified adsorbent.
[0006] By adopting the above technical scheme, the hydrophobic coating uses epoxy resin as the main coating body. The epoxy resin has good hydrophobicity and film-forming properties and can form a hydrophobic coating. Graphene oxide has good flexibility and physical shielding properties for water molecules and air, which can further enhance the hydrophobicity of the coating formed by the hydrophobic coating. The hydrophilic coating uses a hydrophilic modified epoxy resin emulsion, so that the hydrophilic coating can form a hydrophilic epoxy resin coating, which is conducive to absorbing moisture. At the same time, the modified adsorbent can further improve the hydrophilic coating's ability to absorb moisture. The main bodies of the hydrophilic coating and the hydrophobic coating are both epoxy resin, so that the coatings formed by the two have good bonding.
[0007] Preferably, the preparation method of the hydrophilic modified epoxy resin emulsion comprises the following steps: dissolving the epoxy resin in butanol, stirring at 55-60°C for 30-35 minutes, adding diethanolamine dropwise, heating to 78-83°C and keeping the temperature for 5 hours, cooling to 60°C, adding glacial acetic acid for neutralization to make the pH value 7-8, adding deionized water for emulsification under high-speed stirring, and obtaining the hydrophilic modified epoxy resin emulsion.
[0008] By adopting the above technical scheme, diethanolamine is added to carry out a ring-opening reaction with the epoxy group of the epoxy resin, so that hydrophilic groups such as hydroxyl groups and amino groups can be introduced into the epoxy resin, thereby improving the hydrophilicity of the epoxy resin and preparing a hydrophilic modified epoxy resin emulsion.
[0009] Preferably, the preparation method of the modified graphene oxide comprises the following steps: ultrasonically dispersing graphene oxide in a mixture of anhydrous ethanol and water, adding ammonia water while stirring, adjusting the pH to 9-10, adding tetraethoxysilane, reacting for 15-16 hours, centrifuging, washing, ultrasonically dispersing in a mixed solvent of water and ethanol, and freeze-drying to obtain modified graphene oxide.
[0010] By adopting the above technical scheme, after tetraethoxysilane is hydrolyzed, silicon dioxide is deposited on the surface of graphene oxide, so that the surface of graphene oxide is coated with a silicon dioxide layer. Graphene oxide has good conductivity, and silicon dioxide has poor conductivity. After being coated with the silicon dioxide layer, the insulation of the modified graphene oxide is better, which is more suitable for the surface of I-beam used as an electromagnet, and at the same time reduces the promoting effect of graphene oxide on metal corrosion.
[0011] Preferably, the mass ratio of graphene oxide to tetraethoxysilane is (0.8-1.1):(1.7-2.1).
[0012] By adopting the above technical scheme, the mass ratio of graphene oxide to tetraethoxysilane is controlled, so that the silicon dioxide layer deposited on the surface of graphene oxide is more uniform and complete. If the mass ratio of graphene oxide to tetraethoxysilane is too high or too low, the thickness of the silicon dioxide layer may be uneven, resulting in incomplete coating, thereby weakening the shielding effect of the silicon dioxide layer on the conductivity of graphene oxide.
[0013] Preferably, the preparation method of the modified adsorbent comprises the following steps: mixing sodium montmorillonite with water, preparing a suspension by ultrasound, adding sodium alginate while stirring, reacting at 70-80° C. for 3-3.5 hours, drying and grinding to prepare the modified adsorbent.
[0014] By adopting the above technical scheme, sodium montmorillonite has good adsorption properties and can absorb water well. The carboxyl and hydroxyl groups in sodium alginate form hydrogen bonds with the sodium montmorillonite to obtain modified montmorillonite. The modified montmorillonite has a large specific surface area and good water absorption, which improves the interception effect of the hydrophilic coating on water molecules.
[0015] Preferably, the mass ratio of the sodium montmorillonite to sodium alginate is (1.1-1.3):(1.2-1.5).
[0016] By adopting the above technical solution, the mass ratio between sodium montmorillonite and sodium alginate is controlled, and the modification effect of sodium alginate on sodium montmorillonite is optimal, so that the modified adsorbent has the best adsorption and absorption effect on water.
[0017] In a second aspect, the present application provides a method for preparing a rust inhibitor for surface treatment of an I-beam, using the following technical solution: A method for preparing a rust inhibitor for surface treatment of I-beams, including a method for preparing a hydrophobic coating and a method for preparing a hydrophilic coating: The preparation method of the hydrophobic coating comprises the following steps: mixing epoxy resin, filler, dispersant, defoamer, rheological agent, surfactant and modifier, grinding and stirring at a speed of 3000-5000 r / min for 30-40 min, adding water, and fully stirring to obtain the hydrophobic coating; The preparation method of the hydrophilic coating comprises the following steps: mixing a hydrophilic epoxy resin emulsion, a filler, a dispersant, a defoamer, a rheological agent and a surfactant, stirring them uniformly, adding a modified adsorbent and mixing them uniformly to obtain the hydrophilic coating.
[0018] By adopting the above technical scheme, the raw materials of the hydrophobic coating and the hydrophilic coating are evenly mixed through stirring and grinding to prepare the hydrophobic coating and the hydrophilic coating.
[0019] In a third aspect, the present application provides an application of a rust inhibitor for surface treatment of an I-beam, using the following technical solution: The invention discloses an application of a rust preventive for surface treatment of an I-beam, comprising the following steps: spraying a hydrophobic coating on the surface of the I-beam treated by a bluing process, curing at room temperature for 70-74 hours to form a first layer of hydrophobic coating, spraying a hydrophilic coating on the surface of the first layer of hydrophobic coating, curing at 60°C for 4-5 hours to form a hydrophilic coating, spraying the hydrophobic coating on the surface of the hydrophilic coating again, curing at room temperature for 70-74 hours to form a second layer of hydrophobic coating.
[0020] By adopting the above technical scheme, the second layer of hydrophobic coating is located on the outermost side, the hydrophobic coating can effectively intercept water vapor and reduce the contact between the I-beam and water molecules in the environment. The hydrophilic coating and the modified adsorbent can adsorb and absorb the water molecules passing through the second layer of hydrophobic coating. The first layer of hydrophobic coating can further intercept the water molecules. The rust inhibitor can effectively reduce the contact between the I-beam and water molecules, thereby reducing the rust of the I-beam.
[0021] Preferably, the thickness of the first hydrophobic coating layer is 20-30 μm, the thickness of the hydrophilic coating layer is 30-40 μm, and the thickness of the second hydrophobic coating layer is 20-30 μm.
[0022] By adopting the above technical solution, the first layer of hydrophobic coating, the hydrophilic coating and the second layer of hydrophilic coating are controlled, so that the three layers of coating can cooperate with each other, the interception effect of water molecules in the environment is better, the contact between water molecules and the I-beam is reduced, and the rust of the I-beam can be effectively reduced.
[0023] In summary, this application has the following beneficial effects: 1. Since the present application adopts hydrophobic coating and hydrophilic coating, the hydrophobic coating uses epoxy resin as the coating body, epoxy resin has good hydrophobicity and film-forming property, and can form a hydrophobic coating. Graphene oxide has good flexibility and physical shielding properties for water molecules and air, which can further enhance the hydrophobicity of the coating formed by the hydrophobic coating. The hydrophilic coating uses a hydrophilic modified epoxy resin emulsion, so that the hydrophilic coating can form a layer of hydrophilic epoxy resin coating, which is conducive to absorbing moisture. At the same time, the modified adsorbent can further improve the hydrophilic coating's ability to absorb moisture. The main bodies of the hydrophilic coating and the hydrophobic coating are both epoxy resin, so that the coatings formed by the two have good bonding.
[0024] 2. In the present application, modified graphene oxide is preferably used. After tetraethoxysilane is hydrolyzed, silicon dioxide is deposited on the surface of graphene oxide, so that the surface of graphene oxide is coated with a silicon dioxide layer. Graphene oxide has good conductivity, and silicon dioxide has poor conductivity. After being coated with the silicon dioxide layer, the insulation of the modified graphene oxide is better, and it is more suitable for the surface of an I-beam as an electromagnet.
[0025] 3. The method of the present application forms a coating of a hydrophobic-hydrophilic-hydrophobic structure by three spraying steps. The second layer of the hydrophobic coating is located on the outermost side. The hydrophobic coating can effectively intercept water vapor and reduce the contact between the I-beam and water molecules in the environment. The hydrophilic coating and the modified adsorbent can adsorb and absorb the water molecules passing through the second layer of the hydrophobic coating. The first layer of the hydrophobic coating can further intercept the water molecules. The rust inhibitor can effectively reduce the contact between the I-beam and water molecules, thereby reducing the rust of the I-beam. DETAILED DESCRIPTION
[0026] The present application is further described in detail below with reference to the embodiments.
[0027] Preparation Examples 1-4 of Modified Graphene Oxide Preparation Example 1 The preparation method of modified graphene oxide comprises the following steps: ultrasonically dispersing 0.6 g of graphene oxide in 500 mL of a mixed solution of anhydrous ethanol and water in a volume ratio of 9:1, adding 10 wt% ammonia water while stirring, adjusting the pH to 9-10, adding tetraethoxysilane, wherein the mass ratio of graphene oxide to tetraethoxysilane is 0.8:1.7, reacting for 15 hours, centrifuging, washing, ultrasonically dispersing in 100 mL of a mixed solvent of water and ethanol in a volume ratio of 34:1, and freeze-drying to obtain modified graphene oxide.
[0028] Preparation Example 2 The preparation method of modified graphene oxide comprises the following steps: ultrasonically dispersing 0.5 g of graphene oxide in 500 mL of a mixed solution of anhydrous ethanol and water in a volume ratio of 8:1, adding 10 wt% ammonia water while stirring, adjusting the pH to 9-10, adding tetraethoxysilane, wherein the mass ratio of graphene oxide to tetraethoxysilane is 1.1:2.1, reacting for 16 hours, centrifuging, washing, ultrasonically dispersing in 100 mL of a mixed solvent of water and ethanol in a volume ratio of 35:1, and freeze-drying to obtain modified graphene oxide.
[0029] Preparation Example 3 The difference between Preparation Example 3 and Preparation Example 1 is that in Preparation Example 3, the mass ratio of graphene oxide to tetraethoxysilane is 0.8:0.5.
[0030] Preparation Example 4 The difference between Preparation Example 4 and Preparation Example 1 is that in Preparation Example 4, the mass ratio of graphene oxide to tetraethoxysilane is 0.8:2.5.
[0031] Preparation Example 5-8 of Modified Adsorbent Preparation Example 5 The preparation method of the modified adsorbent comprises the following steps: 3 g of sodium montmorillonite is mixed with 97 g of water, ultrasonically treated for 15 min to obtain a suspension, sodium alginate is added while stirring, the mass ratio of sodium montmorillonite to sodium alginate is 1.1:1.2, reacted at 70°C for 3.5 h, dried and ground to obtain the modified adsorbent.
[0032] Preparation Example 6 The preparation method of the modified adsorbent comprises the following steps: mixing 4g of sodium montmorillonite with 96g of water, ultrasonicating for 20min to obtain a suspension, adding sodium alginate while stirring, wherein the mass ratio of sodium montmorillonite to sodium alginate is 1.3:1.5, reacting at 80°C for 3h, drying and grinding to obtain the modified adsorbent.
[0033] Preparation Example 7 The difference between Preparation Example 7 and Preparation Example 5 is that in Preparation Example 7, the mass ratio of sodium montmorillonite to sodium alginate is 1.1:0.5.
[0034] Preparation Example 8 The difference between Preparation Example 8 and Preparation Example 5 is that in Preparation Example 8, the mass ratio of sodium montmorillonite to sodium alginate is 1.1:2.
[0035] Preparation Example 9-10 of Hydrophilic Modified Epoxy Resin Emulsion Preparation Example 9 The preparation method of a hydrophilic modified epoxy resin emulsion comprises the following steps: dissolving 25 g of epoxy resin E-44 in 50 g of butanol, stirring at 60° C. for 30 min, dripping diethanolamine, wherein the molar ratio of ethylene glycolamine to epoxy group is 0.32:1, heating to 78° C. and then keeping the temperature for 5 h, cooling to 60° C. and then adding glacial acetic acid for neutralization to make the pH value be 7, and adding deionized water for emulsification under stirring at 3000 r / min to obtain a hydrophilic modified epoxy resin emulsion, wherein the solid content of the emulsion is 45%.
[0036] Preparation Example 10 The preparation method of a hydrophilic modified epoxy resin emulsion comprises the following steps: dissolving 30 g of epoxy resin E-44 in 60 g of butanol, stirring at 55° C. for 35 min, dripping diethanolamine, wherein the molar ratio of ethylene glycolamine to epoxy group is 0.37:1, heating to 83° C. and then keeping the temperature for 5 h, cooling to 60° C. and then adding glacial acetic acid for neutralization to make the pH value 8, and adding deionized water for emulsification under stirring at 3000 r / min to obtain a hydrophilic modified epoxy resin emulsion, wherein the solid content of the emulsion is 50%. Example
[0037] Example 1 A rust preventive for surface treatment of I-beams, comprising a hydrophobic coating and a hydrophilic coating, wherein the hydrophobic coating comprises 60kg of epoxy resin, 25kg of curing agent, 10kg of filler, 1.5kg of dispersant, 0.2kg of defoamer, 1kg of rheological agent, 0.8kg of surfactant, 1kg of modified graphene oxide and 20kg of water, wherein the epoxy resin is selected from bisphenol A type epoxy resin E-44, purchased from Wuxi Xinyehao Chemical Co., Ltd., the curing agent is selected from epoxy curing agent 593, purchased from Jiangyin Wanqian Chemical Co., Ltd., the filler is selected from talcum powder, purchased from Jiangyin Guangyuan Superfine Powder Co., Ltd., the dispersant model is BYK190, purchased from Guangdong Yongfeng Chemical Co., Ltd., the defoamer model is ZW-0098, purchased from Guangzhou Zhongwan New Materials Co., Ltd., and the rheological agent model is BYK-R 607, purchased from Guangzhou Si Tu Yuan Chemical Co., Ltd., the surfactant is XP-70, purchased from Shanghai Kai Yin Chemical Co., Ltd., and the modified graphene oxide is the modified graphene oxide prepared in Preparation Example 1.
[0038] The hydrophilic coating includes 40kg of hydrophilic modified epoxy resin emulsion, 15kg of curing agent, 8kg of filler, 1.5kg of dispersant, 0.1kg of defoaming agent, 0.5kg of rheological agent, 0.5kg of surfactant, and 0.2kg of modified adsorbent. The hydrophilic modified epoxy resin coating selects the hydrophilic modified epoxy resin emulsion prepared in Preparation Example 9, and the selection of filler, dispersant, defoaming agent, rheological agent, and surfactant is the same as that in the hydrophobic coating. The modified adsorbent selects the modified adsorbent prepared in Preparation Example 5.
[0039] The preparation method of the above-mentioned rust inhibitor for surface treatment of I-beam includes a preparation method of a hydrophobic coating and a preparation method of a hydrophilic coating: The preparation method of the hydrophobic coating comprises the following steps: after mixing the epoxy resin and the filler, grinding and stirring at a speed of 3000r / min for 40min, adding a dispersant, a defoaming agent, a rheological agent, a surfactant, a modifier and water, and fully stirring to obtain the hydrophobic coating; The preparation method of the hydrophilic coating comprises the following steps: mixing a hydrophilic epoxy resin emulsion, a filler, a dispersant, a defoamer, a rheological agent and a surfactant, stirring them uniformly, adding a modified adsorbent and mixing them uniformly to obtain the hydrophilic coating.
[0040] The application of the above-mentioned rust inhibitor for surface treatment of I-beam comprises the following steps: The I-beam was immersed in a 2 mol / L sodium hydroxide solution for 5 minutes for degreasing, and then pickled and rusted with 25 wt % hydrochloric acid. The bluing liquid was mixed with water and diluted 5 times. The I-beam was immersed in the diluted bluing liquid, taken out after soaking for 40 seconds, and dried naturally to complete the bluing process. The bluing liquid was purchased from Xingtai Wei Neng Technology Co., Ltd. and the model was steel room temperature blackening liquid CH108.
[0041] The hydrophobic coating is sprayed on the surface of the I-beam after the bluing process. After curing at room temperature for 70 hours, a first layer of hydrophobic coating is formed. The thickness of the first layer of hydrophobic coating is 20 μm. The hydrophilic coating is sprayed on the surface of the first layer of hydrophobic coating. After curing at 60°C for 5 hours, a hydrophilic coating is formed. The thickness of the hydrophilic coating is 40 μm. The hydrophobic coating is sprayed on the surface of the hydrophilic coating again. After curing at room temperature for 70 hours, a second layer of hydrophobic coating is formed. The thickness of the second layer of hydrophobic coating is 20 μm.
[0042] Example 2 A rust preventive for surface treatment of I-beams, comprising a hydrophobic coating and a hydrophilic coating, wherein the hydrophobic coating comprises 70kg of epoxy resin, 30kg of curing agent, 15kg of filler, 2.5kg of dispersant, 0.6kg of defoamer, 1.5kg of rheological agent, 1.6kg of surfactant, 2.8kg of modified graphene oxide and 35kg of water, wherein the epoxy resin is selected from bisphenol A type epoxy resin E-44, purchased from Wuxi Xinyehao Chemical Co., Ltd., the curing agent is selected from epoxy curing agent 593, purchased from Jiangyin Wanqian Chemical Co., Ltd., the filler is selected from talcum powder, purchased from Jiangyin Guangyuan Superfine Powder Co., Ltd., the dispersant model is BYK190, purchased from Guangdong Yongfeng Chemical Co., Ltd., the defoamer model is ZW-0098, purchased from Guangzhou Zhongwan New Materials Co., Ltd., and the rheological agent model is BYK-R 607, purchased from Guangzhou Si Tu Yuan Chemical Co., Ltd., the surfactant is XP-70, purchased from Shanghai Kai Yin Chemical Co., Ltd., and the modified graphene oxide is the modified graphene oxide prepared in Preparation Example 2.
[0043] The hydrophilic coating includes 50kg of hydrophilic modified epoxy resin emulsion, 20kg of curing agent, 12kg of filler, 3kg of dispersant, 0.4kg of defoamer, 1kg of rheological agent, 1kg of surfactant, and 0.5kg of modified adsorbent, wherein the hydrophilic modified epoxy resin coating selects the hydrophilic modified epoxy resin emulsion prepared in Preparation Example 10, and the selection of filler, dispersant, defoamer, rheological agent, and surfactant is the same as that in the hydrophobic coating, and the modified adsorbent selects the modified adsorbent prepared in Preparation Example 6.
[0044] The preparation method of the above-mentioned rust inhibitor for surface treatment of I-beam includes a preparation method of a hydrophobic coating and a preparation method of a hydrophilic coating: The preparation method of the hydrophobic coating comprises the following steps: after mixing the epoxy resin and the filler, grinding and stirring at a speed of 5000r / min for 30min, adding a dispersant, a defoaming agent, a rheological agent, a surfactant, a modifier and water, and fully stirring to obtain the hydrophobic coating; The preparation method of the hydrophilic coating comprises the following steps: mixing a hydrophilic epoxy resin emulsion, a filler, a dispersant, a defoamer, a rheological agent and a surfactant, stirring them uniformly, adding a modified adsorbent and mixing them uniformly to obtain the hydrophilic coating.
[0045] The application of the above-mentioned rust inhibitor for surface treatment of I-beam comprises the following steps: The I-beam was immersed in a 2 mol / L sodium hydroxide solution for 5 minutes for degreasing, and then pickled and rusted with 25 wt % hydrochloric acid. The bluing liquid was mixed with water and diluted 5 times. The I-beam was immersed in the diluted bluing liquid, taken out after soaking for 40 seconds, and dried naturally to complete the bluing process. The bluing liquid was purchased from Xingtai Wei Neng Technology Co., Ltd. and the model was steel room temperature blackening liquid CH108.
[0046] The hydrophobic coating is sprayed on the surface of the I-beam after the bluing process. After curing at room temperature for 74 hours, a first layer of hydrophobic coating is formed. The thickness of the first layer of hydrophobic coating is 30 μm. The hydrophilic coating is sprayed on the surface of the first layer of hydrophobic coating. After curing at 60°C for 4 hours, a hydrophilic coating is formed. The thickness of the hydrophilic coating is 30 μm. The hydrophobic coating is sprayed on the surface of the hydrophilic coating again. After curing at room temperature for 74 hours, a second layer of hydrophobic coating is formed. The thickness of the second layer of hydrophobic coating is 30 μm.
[0047] Example 3 The difference between Example 3 and Example 1 is that in Example 3, the modified graphene oxide is the modified graphene oxide prepared in Preparation Example 3.
[0048] Example 4 The difference between Example 4 and Example 1 is that in Example 4, the modified graphene oxide is the modified graphene oxide prepared in Preparation Example 4.
[0049] Example 5 The difference between Example 5 and Example 1 is that in Example 5, the modified adsorbent is the modified adsorbent prepared in Preparation Example 7.
[0050] Example 6 The difference between Example 6 and Example 1 is that in Example 6, the modified adsorbent is the modified adsorbent prepared in Preparation Example 8.
[0051] Example 7 The difference between Example 7 and Example 1 is that in Example 7, the modified adsorbent is replaced by an equal amount of sodium montmorillonite, and the sodium montmorillonite model is PGW, which is purchased from Shanghai Jiyi Biotechnology Co., Ltd.
[0052] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the application of the rust inhibitor for the surface treatment of the I-beam includes the following steps: spraying a hydrophobic coating on the surface of the I-beam treated by the bluing process, and curing it at 60°C for 5 hours to form a hydrophilic coating with a thickness of 40 μm. Spraying the hydrophobic coating on the surface of the hydrophilic coating again, and curing it at room temperature for 70 hours to form a second layer of hydrophobic coating with a thickness of 20 μm.
[0053] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the application of the rust inhibitor for the surface treatment of the I-beam includes the following steps: spraying a hydrophobic coating on the surface of the I-beam treated by the bluing process, and curing it at room temperature for 70 hours to form a first layer of hydrophobic coating, the thickness of the first layer of hydrophobic coating is 20 μm, and spraying the hydrophobic coating on the surface of the first layer of hydrophobic coating again, and curing it at room temperature for 70 hours to form a second layer of hydrophobic coating, the thickness of the second layer of hydrophobic coating is 20 μm.
[0054] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the application of the rust inhibitor for the surface treatment of the I-beam includes the following steps: spraying a hydrophobic coating on the surface of the I-beam treated by the bluing process, and curing it at room temperature for 70 hours to form a first layer of hydrophobic coating, and the thickness of the first layer of hydrophobic coating is 20 μm; spraying a hydrophilic coating on the surface of the first layer of hydrophobic coating, and curing it at 60°C for 5 hours to form a hydrophilic coating, and the thickness of the hydrophilic coating is 40 μm.
[0055] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that the application of the rust inhibitor for the surface treatment of the I-beam includes the following steps: spraying the hydrophobic coating on the surface of the I-beam, and curing it at room temperature for 70 hours to form a first layer of hydrophobic coating, and the thickness of the first layer of hydrophobic coating is 20 μm.
[0056] Comparative Example 5 The difference between Comparative Example 5 and Example 1 is that in Comparative Example 5, an equal amount of graphene oxide is used instead of modified graphene oxide.
[0057] Comparative Example 6 The difference between Comparative Example 6 and Example 1 is that in Comparative Example 6, graphene oxide is not added to the hydrophobic coating.
[0058] Comparative Example 7 The difference between Comparative Example 7 and Example 1 is that in Comparative Example 7, no modified adsorbent is added to the hydrophilic coating.
[0059] Detection Methods According to the raw materials and preparation methods of Examples 1-7 and Comparative Examples 1-7, a rust inhibitor for surface treatment of I-beams was prepared, and sprayed according to the method in the application to form a coating film, and the salt spray resistance of the coating film was tested. The salt spray resistance test referred to "GB / T1771-2007 Determination of neutral salt spray resistance of paints and varnishes", and the results were recorded in Table 1.
[0060] Table 1 Neutral salt spray resistance of rust inhibitors According to Table 1, Examples 1-2 and Comparative Examples 1-4, it can be seen that the neutral salt spray resistance of Examples 1-2 is better than that of Comparative Examples 1-4. In Examples 1-2, the hydrophobic coating is sprayed once to form a first layer of hydrophobic coating, and then the hydrophilic coating is sprayed to form a hydrophilic coating. The hydrophobic coating is sprayed twice to form a second layer of hydrophobic coating, and finally a three-layer coating with a hydrophobic-hydrophilic-hydrophobic structure from the inside to the outside is formed. There is no first layer of hydrophobic coating in Comparative Example 1, no hydrophilic coating in Comparative Example 2, no second layer of hydrophobic coating in Comparative Example 3, and only one layer of hydrophobic coating is sprayed in Comparative Example 4, which shows that in Examples 1-2, the coating with a hydrophobic-hydrophilic-hydrophobic structure has a good shielding effect on water molecules, thereby achieving anti-rust protection for the metal.
[0061] The three-layer coating of the hydrophobic-hydrophilic-hydrophobic structure, the second hydrophobic coating located on the outermost side of the coating has good hydrophobicity, and the modified graphene oxide in the hydrophobic coating has good shielding performance for water molecules and air, further improving the interception effect of the second hydrophobic coating on water molecules, so that the second hydrophobic coating can block most of the water from entering; the hydrophilic coating is sprayed with a hydrophilic coating, so that the hydrophilic coating has good hydrophilic properties and can absorb and adsorb water passing through the second hydrophobic coating, and at the same time, a modified adsorbent is added to the hydrophilic coating, and the modified adsorbent has good adsorption performance for water, further improving the absorption and adsorption of water by the hydrophilic coating; the first hydrophobic coating located on the innermost side of the coating and in contact with the metal also has good hydrophobicity, and can intercept and shield the water molecules passing through the hydrophilic coating again, thereby reducing the contact between the metal and water, and further reducing the probability of metal corrosion.
[0062] In Comparative Example 1, the hydrophilic coating is in direct contact with the metal and is located in a humid environment for a long time. The hydrophilic coating absorbs more moisture and loses the shielding and isolation effect of the first layer of hydrophobic coating, which makes it easy for the metal to contact the hydrophilic coating with more moisture and rust; in Comparative Example 2, the coating is composed of two layers of hydrophobic coatings without a hydrophilic coating, so that the coating's absorption and interception effect on moisture is reduced compared with Examples 1-2; in Comparative Example 3, the coating has a hydrophobic-hydrophilic structure from the inside to the outside, and there is no second layer of hydrophobic coating to shield water molecules, so that the anti-corrosion effect of the coating in Comparative Example 3 is reduced; in Comparative Example 4, the coating is a single layer of hydrophobic coating, and it can be seen that the hydrophobic coating has a good shielding effect on moisture and has a better anti-corrosion effect, but compared with the coating with a hydrophobic-hydrophilic-hydrophobic three-layer structure in Examples 1-2, the anti-corrosion effect is slightly reduced.
[0063] Compared with Example 1, the neutral salt spray resistance of Comparative Example 5 is reduced. The graphene oxide in Comparative Example 5 is not modified. Graphene oxide has good electrical conductivity and promotes metal corrosion. A layer of silicon dioxide is formed on the surface of graphene oxide by hydrolysis of tetraethoxysilane. The electrical conductivity of silicon dioxide is poor, which can improve the insulation performance of modified graphene oxide, reduce the promoting effect of graphene oxide on metal corrosion, and improve the anti-corrosion effect of the hydrophobic coating. At the same time, the I-beam, as the core of the electromagnet, needs to have good insulation properties.
[0064] Compared with Example 1, the neutral salt spray resistance of Example 3-4 is reduced. In Example 3-4, the mass ratio of graphene oxide to tetraethoxysilane is changed during the preparation of modified graphene oxide, indicating that the mass ratio of graphene oxide to tetraethoxysilane affects the performance of modified graphene oxide. If the mass ratio of graphene oxide to tetraethoxysilane is too high or too low, the thickness of the silicon dioxide layer deposited on the surface of graphene oxide may be uneven or the coating may be incomplete, thereby weakening the shielding effect of the silicon dioxide layer on the conductivity of graphene oxide, thereby increasing the promoting effect of graphene oxide on metal corrosion, and then reducing the anti-corrosion effect of the hydrophobic coating.
[0065] Compared with Example 1, the neutral salt spray resistance of Example 5-7 is reduced. When preparing the modified adsorbent in Example 5-6, the mass ratio of sodium montmorillonite to sodium alginate was changed, indicating that the mass ratio of sodium montmorillonite to sodium alginate has an impact on the performance of the modified adsorbent. Unmodified sodium montmorillonite is used in Example 7, indicating that the modified sodium montmorillonite has better absorption and adsorption performance for water. Sodium montmorillonite has good adsorption performance. The carboxyl and hydroxyl groups in sodium alginate form hydrogen bonds with sodium montmorillonite to obtain modified montmorillonite, which improves the water absorption of the modified montmorillonite and enhances the adsorption and absorption effect of the hydrophilic coating on water. The mass ratio of sodium montmorillonite to sodium alginate is controlled to make the performance of the modified montmorillonite better, thereby improving the absorption and adsorption effect of the clear water coating on water.
[0066] Compared with Example 1, the neutral salt spray resistance of Example 6-7 is reduced. No modified graphene oxide is added to the hydrophobic coating of Comparative Example 6. The modified graphene oxide has a strong shielding effect on water molecules and air, and can reduce the passage of moisture through the hydrophobic coating. No modified graphene oxide is added in Comparative Example 6, so that the anti-corrosion effect of the hydrophobic coating in Comparative Example 6 is weakened; no modified adsorbent is added to the hydrophilic coating of Comparative Example 7, and the modified adsorbent has a good adsorption and absorption effect on water, so that the hydrophilic coating can effectively absorb and intercept moisture. No modified adsorbent is added in Comparative Example 7, so that the water absorption performance of the hydrophilic coating in Comparative Example 6 is reduced, the interception effect is weakened, and the overall anti-corrosion effect of the coating is reduced.
[0067] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A rust preventive for surface treatment of I-beams, Features: The invention comprises a hydrophobic coating and a hydrophilic coating, wherein the hydrophobic coating comprises 60-70 parts of epoxy resin, 25-30 parts of curing agent, 10-15 parts of filler, 1.5-2.5 parts of dispersant, 0.2-0.6 parts of defoaming agent, 1-1.5 parts of rheological agent, 0.8-1.6 parts of surfactant, 1-2.8 parts of modified graphene oxide and 20-35 parts of water; The hydrophilic coating comprises 40-50 parts of hydrophilic modified epoxy resin emulsion, 15-20 parts of curing agent, 8-12 parts of filler, 1.5-3 parts of dispersant, 0.1-0.4 parts of defoamer, 0.5-1 parts of rheological agent, 0.5-1 parts of surfactant and 0.2-0.5 parts of modified adsorbent.
2. The rust preventive for surface treatment of I-beam according to claim 1, Features: The preparation method of the hydrophilic modified epoxy resin emulsion comprises the following steps: dissolving the epoxy resin in butanol, stirring at 55-60°C for 30-35 minutes, dropping diethanolamine, heating to 78-83°C and then keeping the temperature for 5 hours, cooling to 60°C, adding glacial acetic acid for neutralization to make the pH value be 7-8, adding deionized water for emulsification under high-speed stirring, and preparing the hydrophilic modified epoxy resin emulsion.
3. The rust preventive for surface treatment of I-beam according to claim 1, Features: The preparation method of modified graphene oxide comprises the following steps: ultrasonically dispersing graphene oxide in a mixed solution of anhydrous ethanol and water, adding ammonia water while stirring, adjusting the pH to 9-10, adding tetraethoxysilane, reacting for 15-16 hours, centrifuging, washing, ultrasonically dispersing in a mixed solvent of water and ethanol, and freeze-drying to obtain modified graphene oxide.
4. The rust preventive for surface treatment of I-beam according to claim 3, Features: The mass ratio of the graphene oxide to tetraethoxysilane is (0.8-1.1):(1.7-2.1).
5. The rust preventive for surface treatment of I-beam according to claim 1, Features: The preparation method of the modified adsorbent comprises the following steps: mixing sodium montmorillonite with water, obtaining a suspension by ultrasonication, adding sodium alginate while stirring, reacting at 70-80° C. for 3-3.5 hours, drying and grinding to obtain the modified adsorbent.
6. The rust preventive for surface treatment of I-beam according to claim 5, Features: The mass ratio of the sodium montmorillonite to sodium alginate is (1.1-1.3):(1.2-1.5).
7. A method for preparing a rust inhibitor for surface treatment of I-beam according to any one of claims 1 to 6, Features: Including a method for preparing a hydrophobic coating and a method for preparing a hydrophilic coating: The preparation method of the hydrophobic coating comprises the following steps: after mixing the epoxy resin and the filler, grinding and stirring at a speed of 3000-5000 r / min for 30-40 min, adding a dispersant, a defoamer, a rheological agent, a surfactant, a modifier and water, and fully stirring to obtain the hydrophobic coating; The preparation method of the hydrophilic coating comprises the following steps: mixing a hydrophilic epoxy resin emulsion, a filler, a dispersant, a defoamer, a rheological agent and a surfactant, stirring them uniformly, adding a modified adsorbent and mixing them uniformly to obtain the hydrophilic coating.
8. Use of the rust preventive for surface treatment of I-beams obtained by the method for preparing the rust preventive for surface treatment of I-beams as claimed in claim 7, Features: The method comprises the following steps: spraying a hydrophobic coating on the surface of an I-beam treated by a bluing process, curing at room temperature for 70-74 hours to form a first layer of hydrophobic coating, spraying a hydrophilic coating on the surface of the first layer of hydrophobic coating, curing at 60°C for 4-5 hours to form a hydrophilic coating, spraying the hydrophobic coating on the surface of the hydrophilic coating again, curing at room temperature for 70-74 hours to form a second layer of hydrophobic coating.
9. Use of the rust inhibitor for surface treatment of I-beam according to claim 8, Features: The thickness of the first hydrophobic coating layer is 20-30 μm, the thickness of the hydrophilic coating layer is 30-40 μm, and the thickness of the second hydrophobic coating layer is 20-30 μm.
Citation Information
Patent Citations
Method for preparing aqueous epoxy resin
CN101117377A
Diethanolamine modified epoxy resin emulsion as well as preparation method and application thereof
CN108359348A
Antibacterial dustproof cover material for food and preparation method of antibacterial dustproof cover material
CN109486127A
Composite nano-coating material with hydrophobic and anticorrosive performances, and preparation method and application thereof
CN110205023A
Super-hydrophobic surface with stable gas-liquid interface underwater and preparation method thereof