High-temperature-resistant anti-falling polybutylene terephthalate coating and preparation method thereof

Through the cross-linking of composite modified polybutylene terephthalate and monoethanolamine and KH-602 modified zinc phosphate and calcium silicate auxiliary film forming materials, the existing high-temperature resistant coatings are easily changed in high-temperature environments. The problems of brittleness and poor adhesion improve the wear resistance and corrosion resistance of the coating and extend the service life.

CN118931335APending Publication Date: 2024-11-12ZHEJIANG SHUNYANG NEW MATERIAL TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411003825.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing high-temperature resistant coatings are prone to become brittle and have poor adhesion in high-temperature environments, resulting in reduced protection capabilities and shortened service life. Most of them are solvent-based and unenvironmentally friendly.

Method used

Compound modified polybutylene terephthalate combined with the hydroxyl group of monoethanolamine to form a physical crosslinking, increase the wear resistance of the coating, and use KH-602 modified zinc phosphate and calcium silicate as auxiliary production. Film material eliminates the phase interface between resin and powder, blocks the entry of medium, and improves corrosion and rust resistance.

Benefits of technology

It improves the wear resistance, adhesion and corrosion-resistant properties of the coating, extends the service life, and reduces the peeling and peeling problems of the coating, achieving high temperature resistance, corrosion-resistant and anti-shelf effects.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant anti-falling polybutylene terephthalate coating and a preparation method thereof, and relates to the technical field of coating preparation. Fumaric acid participates in polymerization reaction of polybutylene terephthalate, binary unsaturated acid is introduced, the strength of the coating is improved, then hydroxyl is combined with chlorine of trimethoxychlorosilane, a silicon-containing oligomer is obtained, the durability is improved, silicon-oxygen bonds are polymerized on the basis, the crosslinking degree of molecular chains is improved, the performance of the coating is improved, and the service life of the coating is prolonged. Then, KH-602 modified zinc phosphate and calcium silicate powder are added, a phase interface is eliminated, a medium is prevented from entering, and the high-temperature-resistant, anti-corrosion and anti-falling effects are achieved in cooperation with the anti-corrosion and anti-rust performance of zinc phosphate and the high-temperature-resistant performance of calcium silicate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coating preparation, in particular to a high-temperature resistant and anti-shedding polybutylene terephthalate coating and a preparation method thereof. Background Art

[0002] At present, with the continuous development of my country's modern industry, especially in the petrochemical, energy, metallurgy, new materials and military industries, high-temperature equipment and supporting facilities are used in more and more occasions. However, metal materials are prone to oxidation reaction with oxygen in the air in high-temperature environments, resulting in rust, which gradually loses strength and causes structural defects, becoming a hidden danger of various accidents. Therefore, its surface generally needs to be coated with high-temperature resistant anti-corrosion coatings to prevent oxidation corrosion of metal materials and extend the service life of high-temperature equipment. Domestic high-temperature resistant coatings are still in a stage of rapid development, with a wide variety of types, but most of them are solvent-based high-temperature resistant coatings, which contain many volatile substances and are not environmentally friendly; and the coating becomes brittle after high temperature and cannot adhere well to the substrate, resulting in a decrease in protection ability after high temperature and a shortened service life.

[0003] Polybutylene terephthalate (PBT) is composed of saturated linear molecules connected by rigid benzene rings and flexible fatty alcohol chains. The high geometric regularity and rigidity of its molecular structure give it high mechanical strength, excellent chemical and heat resistance, and good electrical properties. There are no side chains in the PBT molecular structure and the structure is symmetrical, which gives it good crystallinity and a high melting point. Therefore, it is very urgent to invent a polybutylene terephthalate coating that is resistant to high temperatures, corrosion, and shedding. Summary of the invention

[0004] The object of the present invention is to provide a high temperature resistant and anti-shedding polybutylene terephthalate coating and a preparation method thereof, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a high temperature resistant and anti-shedding polybutylene terephthalate coating and a preparation method thereof, wherein the high temperature resistant and anti-shedding polybutylene terephthalate coating comprises composite modified polybutylene terephthalate and auxiliary film-forming materials.

[0006] Furthermore, the composite modified polybutylene terephthalate is prepared from modified polybutylene terephthalate and monoethanolamine.

[0007] Furthermore, the modified polybutylene terephthalate is prepared from 1,4-butanediol, terephthalic acid, fumaric acid and trimethoxysilyl chloride.

[0008] Furthermore, the auxiliary film-forming material is made of KH-602, zinc phosphate and calcium silicate.

[0009] Furthermore, a method for preparing a high temperature resistant and anti-shedding polybutylene terephthalate coating comprises the following preparation steps:

[0010] (1) 4 to 8 parts of fumaric acid, 25 to 50 parts of 1,4-butanediol, and 10 to 20 parts of terephthalic acid are placed in a container, 3 to 6 parts of tetrabutyl titanate are added under stirring at 1000 rpm, and the mixture is reacted at 210 to 230° C. for 4 to 8 hours, followed by the addition of 12 to 24 parts of trimethoxysilyl chloride and 20 to 32 parts of triethylamine, and the reaction is continued for 2 to 6 hours, and then the temperature is raised to 240 to 260° C. and maintained under vacuum for 3 to 7 hours, and then the material is discharged under inert gas protection, cooled, and pelletized to obtain modified polybutylene terephthalate;

[0011] (2) placing 13 to 21 parts of modified polybutylene terephthalate and 20 to 32 parts of monoethanolamine in an internal mixer, kneading for 10 to 30 minutes, and then extruding through an extruder to obtain a composite modified polybutylene terephthalate;

[0012] (3) 12 to 16 parts of zinc phosphate and 13 to 17 parts of calcium silicate are fully dried in an oven at 100 to 110° C. for 8 to 12 hours to remove moisture, then placed in a high-speed mixer and stirred at high speed for 20 to 40 minutes, then 8 to 14 parts of KH-602 ethanol mixed solution are added under low-speed stirring, and then stirred at high speed for 60 to 120 minutes to obtain an auxiliary film-forming material;

[0013] (4) 80 to 120 parts of the composite modified polybutylene terephthalate, 10 to 16 parts of the auxiliary film-forming material, and 8 to 12 parts of diethylene glycol butyl ether are mixed uniformly to obtain a high temperature resistant and anti-shedding polybutylene terephthalate coating.

[0014] Furthermore, the vacuum degree in step (1) is 40-100 Pa.

[0015] Furthermore, the inert gas in step (1) is one or more of nitrogen, helium and argon.

[0016] Furthermore, the banburying temperature in step (2) is 160-170°C.

[0017] Furthermore, in step (3), the high-speed stirring is 1000 r / min, and the low-speed stirring is 200 r / min.

[0018] Furthermore, in step (3), the ratio of KH602 to ethanol is 1:20.

[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0020] The invention uses hydrogen bonding between the hydroxyl group of monoethanolamine and the ester carbonyl group in the modified polybutylene terephthalate to generate a physical crosslinking effect between the polymer chains, thereby improving the wear resistance of the coating. At the same time, the amino group in the monoethanolamine is lipophilic, which effectively prevents the coating from peeling and falling off. Finally, a mixed powder of zinc phosphate and calcium silicate modified by KH-602 is added as an auxiliary film-forming material. When the powder is miscible with the modified polybutylene terephthalate succinate, the interface between the resin and the powder can be eliminated, the medium is blocked from entering, the anti-corrosion effect of the coating is improved, and the anti-corrosion and anti-rust performance of zinc phosphate and the high-temperature resistance of calcium silicate are combined to achieve the effects of high-temperature resistance, corrosion resistance and anti-falling.

[0021] The modified polybutylene terephthalate of the present invention utilizes fumaric acid to participate in the polymerization reaction of polybutylene terephthalate to obtain a hydroxyl-containing oligomer, introduces a dibasic unsaturated acid to increase the flexibility of the molecular chain and improve the strength of the coating, and then relies on the combination of the hydroxyl group and the chlorine group of trimethoxychlorosilane to obtain a silicon-containing composite oligomer, which effectively improves the durability and thermal stability of the material and reduces the problems of cracking and peeling of the coating. On this basis, the silicon-oxygen bond is polymerized to increase the crosslinking degree of the polymer molecular chain, thereby improving the coating performance. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the high temperature resistant and anti-shedding polybutylene terephthalate coating prepared in the following examples are as follows:

[0024] Flexibility: Apply the coatings of the embodiments and comparative examples evenly on the sample, place at room temperature for 7 days after curing, place the sample with the coating surface facing up, close to a fixed shaft rod, and then bend it around the shaft rod to observe whether the coating has cracking, falling off, etc., and record the minimum diameter of the shaft rod without defects.

[0025] Heat-resistant temperature: Take the coating of the embodiment and the comparative example and apply it evenly on the sample. After curing, put it into the DRZ-12 high-temperature furnace. After reaching the set temperature, keep it warm for one hour. After cooling to room temperature, observe the surface morphology of the coating and record the lowest temperature without cracking and other problems.

[0026] Adhesion: The coatings of the embodiments and comparative examples were evenly coated on the sample. After curing, the coating film was cut with a cutting tool, and then adhered with adhesive tape and then torn off to observe the peeling of the coating.

[0027] Salt spray resistance: The coatings of the embodiments and comparative examples were evenly coated on the sample plates, and after curing, the test was performed in accordance with GB / T1771-1991.

[0028] Example 1

[0029] (1) 4 parts of fumaric acid, 25 parts of 1,4-butanediol, and 10 parts of terephthalic acid are placed in a container, 3 parts of tetrabutyl titanate are added under stirring at 1000 rpm, and the mixture is reacted at 210° C. for 4 hours, followed by the addition of 12 parts of trimethoxysilyl chloride and 20 parts of triethylamine. The mixture is reacted for 2 hours, and then the temperature is raised to 240° C. and maintained at a vacuum degree of 40 Pa for 3 hours. The mixture is then discharged under helium protection, cooled, and pelletized to obtain modified polybutylene terephthalate;

[0030] (2) placing 13 parts of modified polybutylene terephthalate and 20 parts of monoethanolamine in an internal mixer at 160° C. for 10 minutes and then extruding through an extruder to obtain a composite modified polybutylene terephthalate;

[0031] (3) 12 parts of zinc phosphate and 13 parts of calcium silicate were fully dried in an oven at 100°C for 8 hours to remove moisture, then placed in a high-speed mixer and stirred at 1000 r / min for 20 minutes, then 8 parts of a mixture of KH-602 and ethanol in a ratio of 1:20 were added under stirring at 200 r / min, and then stirred at 1000 r / min for 60 minutes to obtain an auxiliary film-forming material;

[0032] (4) 80 parts of composite modified polybutylene terephthalate, 10 parts of auxiliary film-forming materials, and 8 parts of diethylene glycol butyl ether are mixed uniformly to obtain a high-temperature resistant and anti-shedding polybutylene terephthalate coating.

[0033] Example 2

[0034] (1) 6 parts of fumaric acid, 38 parts of 1,4-butanediol, and 15 parts of terephthalic acid are placed in a container, 4.5 parts of tetrabutyl titanate are added under stirring at 1000 rpm, and the mixture is reacted at 220° C. for 6 hours, followed by adding 18 parts of trimethoxysilyl chloride and 26 parts of triethylamine, and the mixture is reacted for 4 hours, and then the temperature is raised to 250° C. and maintained at a vacuum degree of 70 Pa for 5 hours, and then the mixture is discharged under nitrogen protection, cooled, and pelletized to obtain modified polybutylene terephthalate;

[0035] (2) placing 17 parts of modified polybutylene terephthalate and 26 parts of monoethanolamine in an internal mixer at 165° C. for 20 minutes and then extruding through an extruder to obtain a composite modified polybutylene terephthalate;

[0036] (3) 14 parts of zinc phosphate and 15 parts of calcium silicate were fully dried in an oven at 105°C for 10 hours to remove moisture, then placed in a high-speed mixer and stirred at 1000 r / min for 30 minutes, then 11 parts of a mixture of KH-602 and ethanol in a ratio of 1:20 were added at 200 r / min, and then stirred at 1000 r / min for 90 minutes to obtain an auxiliary film-forming material;

[0037] (4) 100 parts of the composite modified polybutylene terephthalate, 13 parts of the auxiliary film-forming material, and 10 parts of diethylene glycol butyl ether are mixed uniformly to obtain a high-temperature resistant and anti-shedding polybutylene terephthalate coating.

[0038] Example 3

[0039] (1) 8 parts of fumaric acid, 50 parts of 1,4-butanediol, and 20 parts of terephthalic acid are placed in a container, 6 parts of tetrabutyl titanate are added under stirring at 1000 rpm, and the mixture is reacted at 230° C. for 8 hours, followed by adding 24 parts of trimethoxysilyl chloride and 32 parts of triethylamine. The mixture is reacted for 6 hours, and then the temperature is raised to 260° C. and maintained at a vacuum degree of 100 Pa for 7 hours. The mixture is then discharged under argon protection, cooled, and pelletized to obtain modified polybutylene terephthalate;

[0040] (2) placing 21 parts of modified polybutylene terephthalate and 32 parts of monoethanolamine in an internal mixer at 170° C. for 30 minutes and then extruding through an extruder to obtain a composite modified polybutylene terephthalate;

[0041] (3) 16 parts of zinc phosphate and 17 parts of calcium silicate were fully dried in an oven at 110° C. for 12 hours to remove moisture, then placed in a high-speed mixer and stirred at 1000 r / min for 40 minutes, then 14 parts of a mixture of KH-602 and ethanol in a ratio of 1:20 were added under stirring at 200 r / min, and then stirred at 1000 r / min for 120 minutes to obtain an auxiliary film-forming material;

[0042] (4) 120 parts of composite modified polybutylene terephthalate, 16 parts of auxiliary film-forming materials, and 12 parts of diethylene glycol butyl ether are mixed evenly to obtain a high-temperature resistant and anti-shedding polybutylene terephthalate coating.

[0043] Comparative Example 1

[0044] The difference between Comparative Example 1 and Example 2 is only the difference in step (1), and step (1) is modified as follows: 6 parts of fumaric acid, 38 parts of 1,4-butanediol, and 15 parts of terephthalic acid are placed in a container, 4.5 parts of tetrabutyl titanate are added under stirring, and the mixture is reacted at 220° C. for 6 hours, followed by the addition of 18 parts of trimethoxysilyl chloride and 26 parts of triethylamine, and the mixture is reacted for 4 hours, and then the mixture is heated to 250° C. and maintained at a vacuum of 70 Pa for 5 hours, and then the mixture is discharged under nitrogen protection, cooled, and pelletized to obtain modified polybutylene terephthalate. The remaining preparation steps are the same as those in Example 2.

[0045] Comparative Example 2

[0046] The difference between Comparative Example 2 and Example 2 is only the difference in step (1), and step (1) is modified as follows: 6 parts of fumaric acid, 38 parts of 1,4-butanediol, and 15 parts of terephthalic acid are placed in a container, 4.5 parts of tetrabutyl titanate are added under stirring, and the mixture is reacted at 220° C. for 6 hours, followed by the addition of 18 parts of trimethoxysilyl chloride and 26 parts of triethylamine, and the mixture is reacted for 4 hours, and then the mixture is heated to 250° C. and maintained at a vacuum of 70 Pa for 5 hours, and then the mixture is discharged under nitrogen protection, cooled, and pelletized to obtain modified polybutylene terephthalate. The remaining preparation steps are the same as those in Example 2.

[0047] Comparative Example 3

[0048] The difference between Comparative Example 3 and Example 2 is that there is no step (2). The remaining preparation steps are the same as those of Example 2.

[0049] Comparative Example 4

[0050] The difference between Comparative Example 4 and Example 2 is only the difference in step (3), which is modified as follows: 14 parts of zinc phosphate and 17 parts of calcium silicate are fully dried in an oven at 105° C. for 10 hours to remove moisture, thereby obtaining an auxiliary film-forming material. The remaining preparation steps are the same as those in Example 2.

[0051] Comparative Example 5

[0052] The difference between Comparative Example 5 and Example 2 is that step (3) is omitted and step (4) is changed to: 120 parts of the composite modified polybutylene terephthalate and 12 parts of diethylene glycol butyl ether are mixed uniformly to obtain a high temperature resistant and anti-shedding polybutylene terephthalate coating. The remaining preparation steps are the same as those of Example 2.

[0053] Effect example

[0054] Table 1 below shows the performance analysis results of the high temperature resistant and anti-shedding polybutylene terephthalate coatings of Examples 1 to 3 of the present invention and Comparative Examples 1 to 5.

[0055] Flexibility / mm Heat resistance temperature / ℃ Adhesion Salt spray resistance / h Example 1 0.5 650 Complete without shedding 268 Example 2 0.5 650 Complete without shedding 271 Example 3 0.5 650 Complete without shedding 263 Comparative Example 1 2.5 500 Slight shedding 249 Comparative Example 2 2.5 450 Slight shedding 252 Comparative Example 3 1.5 500 Shedding 247 Comparative Example 4 2 400 Moderate shedding 215 Comparative Example 5 1.5 300 Slight shedding 180

[0056] From the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 1, it can be found that the dibasic unsaturated acid participates in the polymerization reaction of polybutylene terephthalate, increases the flexibility of the molecular chain, and improves the strength of the coating; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 2, it can be found that the chlorine group of trimethoxysilyl chloride is combined with the hydroxyl group of the oligomer to form a stable Si-OR bond, thereby increasing the crosslinking degree of the polymer molecular chain and improving the coating performance; from the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 3, it can be found that the hydroxyl group of monoethanolamine is combined with the modified polybutylene terephthalate The ester carboxyl hydrogen bonds are bonded to the polymer chains to produce physical crosslinking, thereby improving the adhesion of the coating. From the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 4, it can be found that the zinc phosphate and calcium silicate powders modified by the aminosilane coupling agent have good hydrophilicity, can eliminate the phase interface between the resin and the powder, block the entry of the medium, and improve the corrosion resistance. From the comparison of the experimental data of Examples 1, 2, and 3 with Comparative Example 5, it can be found that the addition of zinc phosphate provides the Zn element to the coating, and a dense passivation film is formed during corrosion to avoid further corrosion. The addition of calcium silicate enables the coating to obtain better heat resistance.

[0057] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A high temperature resistant and anti-shedding polybutylene terephthalate coating, characterized in that: The high temperature resistant and anti-shedding polybutylene terephthalate coating comprises composite modified polybutylene terephthalate and auxiliary film-forming materials.

2. The high temperature resistant and anti-shedding polybutylene terephthalate coating according to claim 1, characterized in that: The composite modified polybutylene terephthalate is prepared from modified polybutylene terephthalate and monoethanolamine.

3. The high temperature resistant and anti-shedding polybutylene terephthalate coating according to claim 2, characterized in that: The modified polybutylene terephthalate is prepared from 1,4-butanediol, terephthalic acid, fumaric acid and trimethoxysilyl chloride.

4. The high temperature resistant and anti-shedding polybutylene terephthalate coating according to claim 1, characterized in that: The auxiliary film-forming material is made of KH-602, zinc phosphate and calcium silicate.

5. A method for preparing a high temperature resistant and anti-shedding polybutylene terephthalate coating, characterized in that: The method comprises the following preparation steps: (1) 4 to 8 parts of fumaric acid, 25 to 50 parts of 1,4-butanediol, and 10 to 20 parts of terephthalic acid are placed in a container, 3 to 6 parts of tetrabutyl titanate are added under stirring at 1000 rpm, and the mixture is reacted at 210 to 230° C. for 4 to 8 hours, followed by the addition of 12 to 24 parts of trimethoxysilyl chloride and 20 to 32 parts of triethylamine, and the reaction is continued for 2 to 6 hours, and then the temperature is raised to 240 to 260° C. and maintained under vacuum for 3 to 7 hours, and then the material is discharged under inert gas protection, cooled, and pelletized to obtain modified polybutylene terephthalate; (2) placing 13 to 21 parts of modified polybutylene terephthalate and 20 to 32 parts of monoethanolamine in an internal mixer, kneading for 10 to 30 minutes, and then extruding through an extruder to obtain a composite modified polybutylene terephthalate; (3) 12 to 16 parts of zinc phosphate and 13 to 17 parts of calcium silicate are fully dried in an oven at 100 to 110° C. for 8 to 12 hours to remove moisture, then placed in a high-speed mixer and stirred at high speed for 20 to 40 minutes, then 8 to 14 parts of KH-602 ethanol mixed solution are added under low-speed stirring, and then stirred at high speed for 60 to 120 minutes to obtain an auxiliary film-forming material; (4) 80 to 120 parts of the composite modified polybutylene terephthalate, 10 to 16 parts of the auxiliary film-forming material, and 8 to 12 parts of diethylene glycol butyl ether are mixed uniformly to obtain a high temperature resistant and anti-shedding polybutylene terephthalate coating.

6. The method for preparing a high temperature resistant and anti-shedding polybutylene terephthalate coating according to claim 5, characterized in that: The vacuum degree in step (1) is 40-100 Pa.

7. The method for preparing a high temperature resistant and anti-shedding polybutylene terephthalate coating according to claim 5, characterized in that: The inert gas in step (1) is one or more of nitrogen, helium and argon.

8. The method for preparing a high temperature resistant and anti-shedding polybutylene terephthalate coating according to claim 5, characterized in that: The banburying temperature in step (2) is 160-170°C.

9. The method for preparing a high temperature resistant and anti-shedding polybutylene terephthalate coating according to claim 5, characterized in that: The high-speed stirring in step (3) is 1000 r / min, and the low-speed stirring is 200 r / min.

10. The method for preparing a high temperature resistant and anti-shedding polybutylene terephthalate coating according to claim 5, characterized in that: In step (3), the ratio of KH-602 to ethanol is 1:20.

Citation Information

Patent Citations

  • Jar coating composition

    CN101037565A

  • PBT copolyester with high glass transition temperature and low melting point and application thereof

    CN114479030A

  • Biodegradable PBAT color master batch and fiber prepared from same

    CN115403904A

  • Organic silicon modified water-based paint and preparation method thereof

    CN118085661A

  • Resin composition, molded article, composite, and metal-resin composite

    CN118318007A