Amino-terminated silane coupling agent-terminated high-temperature-resistant coating as well as preparation method and application thereof

By adding end aminosilane coupling agent to polyimide coatings to build chemical bonds, the problem of insufficient adhesion and temperature resistance of polyimide coatings is solved, and effective protection in high-temperature environments and material life is achieved.

CN118931371APending Publication Date: 2024-11-12HARBIN INST OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411117685.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Polyimide coatings have weak adhesion and low temperature resistance, so they cannot be used for a long time in high temperature environments of 450℃ or above.

Method used

The preparation method of high-temperature resistant coating with end-aminosilane coupling agent is adopted to dissolve diamines and dianhydrides in polar aprotic solvents under nitrogen protection to form polyamic acid, and then the end-aminosilane coupling agent is added to construct chemical bonds. Enhance adhesion strength and high temperature resistance.

Benefits of technology

It realizes effective protection of metal devices in a high temperature environment above 450°C, extends the service life of the material, and the coating is non-toxic and harmless, self-extinguishing, low-cost and easy to industrialize.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931371A_ABST
    Figure CN118931371A_ABST
Patent Text Reader

Abstract

The invention provides amino-terminated silane coupling agent-terminated high-temperature-resistant paint as well as a preparation method and application thereof, and relates to the technical field of paint preparation. The preparation method of the amino-terminated silane coupling agent-terminated high-temperature-resistant coating comprises the following steps: dissolving diamine in a polar aprotic solvent to prepare a diamine solution; adding dianhydride into the diamine solution to obtain polyamide acid; and adding the amino-terminated silane coupling agent into the polyamide acid to obtain the amino-terminated silane coupling agent terminated high-temperature-resistant coating. An amino-terminated silane coupling agent is used for blocking, a chemical bond between an inorganic base material and a polyimide coating is constructed by utilizing a silanol bond obtained by hydrolysis in the silane coupling agent and two different characteristic groups of amino-terminated groups, and thermal degradation of a polyamide acid matrix is retarded by utilizing a self rigid structure, so that excellent strong and tough adhesive strength is obtained, the protective capability is excellent, and the service life of the coating is prolonged. The high-temperature resistance of the coating is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of coating preparation, and in particular to a high temperature resistant coating terminated with an amino-terminated silane coupling agent, and a preparation method and application thereof. Background Art

[0002] With the development of technology, the working temperature of metal structural parts is getting higher and higher. In a high-temperature working environment, metal structural parts are facing high-temperature ablation and aging, which can easily cause serious damage to metal structural parts and bring dangers. It will also interrupt operations and lead to a large number of asset repairs and replacements. At present, in order to meet the requirements of miniaturization and lightweight, the size and circuit system of a large number of products are very compact. In order to provide space for the assembly of parts, applying a high-temperature resistant coating is a very advantageous protective means. High-temperature resistant coatings are generally flame-retardant or non-combustible materials. When heat accumulates, it can prevent the protected substrate from direct contact with air and fire sources, thereby playing a protective role. Most of the commonly used high-temperature resistant coatings on the market are inorganic coatings, which have high density, uneven coverage, easy cracking at high temperatures, high prices, limited colors, and harmful and toxic heavy metals. At this stage, most organic high-temperature resistant coatings are silicone resins or modified silicone resins, but silicone resins have poor corrosion resistance and adhesion. Polyimide coatings have the characteristics of good thermal stability, radiation resistance, excellent mechanical properties, low dielectric properties and flame retardancy due to the presence of a five-membered imide ring (-CO-N-CO-) in their main chain. They are widely used in aerospace, military, civil industry, microelectronics and other fields. However, polyimide coatings currently have weak adhesion and low temperature resistance of about 350°C. They cannot be used in working environments of 450°C and above, or can only be used instantaneously and cannot be used for a long time. Summary of the invention

[0003] The problem solved by the invention is how to solve the problem that the polyimide coating has weak adhesion and low temperature resistance.

[0004] In order to solve the above problems, the present invention provides a high temperature resistant coating terminated with an amino-terminated silane coupling agent, and a preparation method and application thereof.

[0005] In a first aspect, the present invention provides a method for preparing a high temperature resistant coating terminated with an amino-terminated silane coupling agent, comprising the following steps:

[0006] S1: Under nitrogen protection, diamine is dissolved in a polar aprotic solvent to prepare a diamine solution with a concentration of 20%wt;

[0007] S2: adding dianhydride to the diamine solution in multiple portions, mixing and reacting for more than 6 hours to obtain polyamic acid;

[0008] S3: Adding an amino-terminated silane coupling agent to the polyamic acid and continuing the reaction for more than 2 hours to obtain a high temperature resistant coating capped with the amino-terminated silane coupling agent.

[0009] Optionally, step S3 specifically includes: adding an amino-terminated silane coupling agent to a polar aprotic solvent, dissolving and dispersing for more than 20 minutes to obtain an amino-terminated silane coupling agent solution, adding the amino-terminated silane coupling agent solution dropwise to polyamic acid, and continuing the reaction for more than 2 hours to obtain a high-temperature resistant coating capped with an amino-terminated silane coupling agent.

[0010] Optionally, the polar aprotic solvent is any one of N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO).

[0011] Optionally, the diamine is one or more of 2-(4-aminophenyl)-5-aminobenzoxazole, 9,9-bis(3-fluoro-4-aminophenyl)fluorene, and 2,2′-bis(trifluoromethyl)-(1,1′-diphenyl)-4,4′-diamine.

[0012] Optionally, the dianhydride is an aromatic dianhydride, and the aromatic dianhydride is one or more of 2,3,3',4'-biphenyltetracarboxylic dianhydride, pyromellitic dianhydride or hexafluorodianhydride.

[0013] Optionally, the amino-terminated silane coupling agent is one or more of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane or γ-aminopropylmethyldimethoxysilane.

[0014] Optionally, the amount of the amino-terminated silane coupling agent added is 1%-5% of the total solid mass of the diamine and the dianhydride.

[0015] Optionally, the molar ratio of the added amounts of diamine and dianhydride is 1:1.

[0016] In a second aspect, the present invention provides a high temperature resistant coating terminated with an amino-terminated silane coupling agent, which is prepared by the preparation method of the high temperature resistant coating terminated with an amino-terminated silane coupling agent as described in any one of the above items.

[0017] In a third aspect, the present invention provides an application of the above-mentioned high-temperature resistant coating terminated with a terminal amino silane coupling agent, which is applied on a stainless steel plate and placed in an oven for high-temperature curing.

[0018] The beneficial effects of the high-temperature resistant coating capped with an amino-terminated silane coupling agent of the present invention and its preparation method and application are as follows: the amino-terminated silane coupling agent is used for capping, and the chemical bond between the inorganic substrate and the polyimide coating is constructed by utilizing the silanol bond obtained by hydrolysis in the silane coupling agent and the two different characteristic groups of the amino group, and the self-rigid structure is utilized to slow down the thermal degradation of the polyamic acid matrix, thereby obtaining excellent strong and tough adhesion strength, excellent protective ability, and enhanced high-temperature resistance of the coating. The coating preparation process is simple, the raw material cost is low, and it is easy to industrialize. The obtained coating is non-toxic and harmless and has self-extinguishing properties, and can effectively protect metal devices in a high-temperature environment above 450°C, reduce high-temperature aging of metal devices to extend the service life of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic diagram of a finished product of a layer formed by brushing a high temperature resistant coating capped with an amino-terminated silane coupling agent in this embodiment;

[0020] Figure 2 This is a schematic diagram of a layer formed by brushing a high temperature resistant coating capped with an amino-terminated silane coupling agent in this embodiment after being ablated at 450° C. for five hours;

[0021] Figure 3 This is a test diagram of the adhesion of a layer formed by brushing the high temperature resistant coating capped with the amino-terminated silane coupling agent of this embodiment;

[0022] Figure 4 This is a graph showing the adhesion of a layer of a high temperature resistant coating blocked with an amino-terminated silane coupling agent in this embodiment after being ablated at 450° C. for five hours;

[0023] Figure 5 This is a scanning electron microscope image of a layer formed by brushing the high temperature resistant coating capped with the amino-terminated silane coupling agent of this embodiment after ablation at 450° C. for five hours. DETAILED DESCRIPTION

[0024] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.

[0025] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;

[0026] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.

[0027] In view of the problems existing in the above-mentioned related technologies, this embodiment provides a high-temperature resistant coating capped with a terminal amino silane coupling agent, and a preparation method and application thereof.

[0028] The present invention provides a method for preparing a high temperature resistant coating capped with an amino-terminated silane coupling agent, comprising the following steps:

[0029] S1: Under nitrogen protection, diamine is dissolved in a polar aprotic solvent to prepare a diamine solution with a concentration of 20%wt;

[0030] S2: adding dianhydride to the diamine solution in multiple portions, mixing and reacting for more than 6 hours to obtain polyamic acid;

[0031] S3: Adding an amino-terminated silane coupling agent to the polyamic acid and continuing the reaction for more than 2 hours to obtain a high temperature resistant coating capped with the amino-terminated silane coupling agent.

[0032] Specifically, in step S2, dianhydride is added in four times for reaction, half of the remaining amount is added in one time, and all of the remaining amount is added in the fourth time.

[0033] In this embodiment, an amino-terminated silane coupling agent is used for end-capping, and the chemical bond between the inorganic substrate and the polyimide coating is constructed by utilizing the two different characteristic groups, namely the silanol bond obtained by hydrolysis in the silane coupling agent and the amino-terminated group. The rigid structure thereof is utilized to slow down the thermal degradation of the polyamic acid matrix, thereby obtaining excellent strong and tough adhesion strength, excellent protective capability, and enhanced high temperature resistance of the coating. The coating preparation process is simple, the raw material cost is low, and it is easy to industrialize. The obtained coating is non-toxic, harmless, and self-extinguishing, and can effectively protect metal devices in a high temperature environment above 450°C, reduce high temperature aging of metal devices, and extend the service life of the material.

[0034] Specifically, Figure 2 and Figure 5 As shown, the high temperature resistant coating terminated with terminal amino silane coupling agent has no shedding, blistering or cracking after being ablated at 450 degrees Celsius for five hours. It has excellent adhesion strength, strong and tough mechanical strength, low toxicity and self-extinguishing ability.

[0035] Optionally, step S3 specifically includes: adding an amino-terminated silane coupling agent to a polar aprotic solvent, dissolving and dispersing for more than 20 minutes to obtain an amino-terminated silane coupling agent solution, adding the amino-terminated silane coupling agent solution dropwise to polyamic acid, and continuing the reaction for more than 2 hours to obtain a high-temperature resistant coating capped with an amino-terminated silane coupling agent.

[0036] In this optional embodiment, the silane coupling agent is selected from a class of silane coupling agents containing terminal amino groups so that it can be connected to the dianhydride during the reaction. The terminal amino silane coupling is added as a capping agent at the end of the reaction. Before adding, it is stirred, dissolved and dispersed in a polar aprotic solvent for half an hour to facilitate rapid dispersion into the polyamic acid. It is then slowly added dropwise to the prepared polyamic acid with a pipette, and stirring is continued to obtain a polyimide coating capped with a fully reacted silane coupling agent.

[0037] Optionally, the polar aprotic solvent is any one of N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO).

[0038] Optionally, the diamine is one or more of 2-(4-aminophenyl)-5-aminobenzoxazole (AAB), 9,9-bis(3-fluoro-4-aminophenyl)fluorene (FDA), and 2,2'-bis(trifluoromethyl)-(1,1'-diphenyl)-4,4'-diamine (TFMB).

[0039] Optionally, the dianhydride is an aromatic dianhydride, and the aromatic dianhydride is one or more of 2,3,3',4'-biphenyltetracarboxylic dianhydride (α-BPDA), pyromellitic dianhydride (PMDA) or hexafluorodianhydride (6FDA).

[0040] Optionally, the amino-terminated silane coupling agent is one or more of γ-aminopropyltriethoxysilane (KH-550), γ-aminopropyltrimethoxysilane (KH-540), γ-aminopropylmethyldiethoxysilane (JH-M902) or γ-aminopropylmethyldimethoxysilane (KH-554).

[0041] Optionally, the amount of the amino-terminated silane coupling agent added is 1%-5% of the total solid mass of the diamine and the dianhydride.

[0042] Optionally, the molar ratio of the added amounts of diamine and dianhydride is 1:1.

[0043] Specifically, the molar amount of 2,3,3',4'-biphenyltetracarboxylic dianhydride (α-BPDA) is 0-30% of the molar amount of the aromatic diamine, the molar amount of pyromellitic dianhydride (PMDA) is 20%-100% of the molar amount of the aromatic diamine or the molar amount of hexafluorodianhydride (6FDA) is 0%-50% of the molar amount of the aromatic diamine, the molar amount of 2-(4-aminophenyl)-5-aminobenzoxazole (AAB) is 0-80% of the molar amount of the aromatic diamine, and the sum of the molar amounts of 9,9-bis(3-fluoro-4-aminophenyl)fluorene (FDA) and 2,2'-bis(trifluoromethyl)-(1,1'-diphenyl)-4,4'-diamine (TFMB) is 98%-103% of the molar amount of the aromatic diamine.

[0044] In this optional embodiment, after the diamine and dianhydride are completely reacted to generate polyamic acid, no diamine and dianhydride remain in the solution.

[0045] An embodiment of the present invention provides a high-temperature resistant coating capped with a terminal amino silane coupling agent, which is prepared by the preparation method of the high-temperature resistant coating capped with a terminal amino silane coupling agent as described in any one of the above items.

[0046] like Figure 1 As shown, in this embodiment, the high temperature resistant coating terminated with the terminal amino silane coupling agent has excellent strong and tough adhesion strength, excellent protection ability, strong high temperature resistance of the coating, and the obtained coating is non-toxic and harmless and has self-extinguishing properties.

[0047] An application of the high temperature resistant coating capped with a terminal amino silane coupling agent as described above provided in an embodiment of the present invention is applied on a stainless steel plate and placed in an oven for high temperature curing.

[0048] Specifically, the high temperature curing procedure is: 80°C, 2h; 120°C, 2h; 150°C, 2h; 180°C, 2h; 210°C, 2h; 240°C, 2h; 280°C, 1h.

[0049] Optionally, the stainless steel plate is pre-treated: When the stainless steel plate is tested, the surface oil and partial rust will cause the adhesion between the coating and the stainless steel surface to decrease, and it is easy to fall off, crack and bubble during high-temperature ablation, so pre-treatment is required. The commonly selected method is grinding, sandblasting or acid and alkali corrosion. Sandpaper grinding is relatively safer and simple to operate. The specific operation is as follows:

[0050] A stainless steel metal plate of 10cm*5cm*2mm was selected for the experiment. Sandpaper with a grit size of 100-200 was used to grind it in a unidirectional direction at an angle of 45° until the surface became a uniform silver-white color. After grinding, it was immersed in alcohol and ultrasonically treated for 20-30 minutes to remove the fine particles remaining on the surface. Finally, it was cleaned with distilled water and alcohol, and dried at 80°C for later use.

[0051] The present invention is further described below in conjunction with specific embodiments.

[0052] Example 1, Preparation of high temperature resistant coating terminated with amino-terminated silane coupling agent

[0053] Under nitrogen protection, 225.246 g (1 mol) of 2-(4-aminophenyl)-5-aminobenzoxazole (AAB) was dissolved in 2300 g of DMAc at room temperature, and 236.13 g (1 mol) of pyromellitic anhydride (PMDA) was added in four batches. After stirring for 6 hours, 1% wt of γ-aminopropylmethyldimethoxysilane uniformly dispersed in a polar aprotic solvent was added. After mixing evenly, stirring was continued for 2 hours, and the stirring polymerization temperature was kept not exceeding room temperature. After mixing evenly, it was coated on a stainless steel substrate and placed in an oven for high-temperature curing to obtain a high-temperature resistant thermoplastic polyimide coating.

[0054] Example 2, Preparation of high temperature resistant coating capped with amino-terminated silane coupling agent

[0055] Under nitrogen protection, 348.44 g (1 mol) of 9,9-bis (3-fluoro-4-aminophenyl) fluorene (FDA) was dissolved in 3200 g of DMAc at room temperature, and 118.07 g (0.5 mol) of pyromellitic anhydride (PMDA) and 174.22 g (0.5 mol) of 2,3,3',4'-biphenyltetracarboxylic anhydride (α-BPDA) were added in four batches. After stirring for 6 hours, 2% wt of γ-aminopropylmethyldiethoxysilane uniformly dispersed in a polar aprotic solvent was added, and the mixture was mixed and stirred for 2 hours. The stirring polymerization temperature was kept at no more than room temperature, and the obtained polyamic acid was coated on a stainless steel substrate, and placed in an oven for high-temperature curing to obtain a high-temperature resistant thermoplastic polyimide coating.

[0056] Example 3, Preparation of high temperature resistant coating terminated with amino-terminated silane coupling agent

[0057] Under nitrogen protection, 224.16 g (0.7 mol) of 2,2'-bis(trifluoromethyl)-(1,1'-diphenyl)-4,4'-diamine (TFMB) and 67.57 g (0.3 mol) of 2-(4-aminophenyl)-5-aminobenzoxazole (AAB) were dissolved in 2600 g of DMAc at room temperature, and 236.13 g (1.0 mol) of pyromellitic dianhydride (PMDA) was added in four batches. After stirring for 6 hours, 3% wt of γ-aminopropyltriethoxysilane uniformly dispersed in a polar aprotic solvent was added. After mixing evenly, stirring was continued for 2 hours, and the stirring polymerization temperature was kept at no more than room temperature. The obtained polyamic acid was coated on a stainless steel substrate, and placed in an oven for high-temperature curing to obtain a high-temperature resistant thermoplastic polyimide coating.

[0058] Example 4: Preparation of high temperature resistant coating terminated with amino-terminated silane coupling agent

[0059] Under nitrogen protection, 320.23g (1 mol) of 2,2'-bis(trifluoromethyl)-(1,1'-diphenyl)-4,4'-diamine (TFMB) was dissolved in 20g of DMAc at room temperature, and 118.07g (0.5mol) of pyromellitic anhydride (PMDA) and 174.22g (0.5mol) of 2,3,3',4'-biphenyltetracarboxylic anhydride (α-BPDA) were added in four batches. After stirring for 6 hours, 5%wt of γ-aminopropyltrimethoxysilane uniformly dispersed in a polar aprotic solvent was added, and the mixture was stirred for 2 hours after being evenly mixed. The stirring polymerization temperature was kept at no more than room temperature, and the obtained polyamic acid was coated on a stainless steel substrate, and then placed in an oven for high-temperature curing to obtain a high-temperature resistant thermoplastic polyimide coating.

[0060] Example 5, Preparation of high temperature resistant coating terminated with amino-terminated silane coupling agent

[0061] Under nitrogen protection, 69.69 g (0.2 mol) of 9,9-bis (3-fluoro-4-aminophenyl) fluorene (FDA) and 180.20 g (0.8 mol) of 2- (4-aminophenyl) -5-aminobenzoxazole (AAB) were dissolved in 20 g of DMAc at room temperature, and 236.14 g (1 mol) of pyromellitic dianhydride (PMDA) was added in four batches. After stirring for 6 hours, 5% wt of γ-aminopropyltrimethoxysilane uniformly dispersed in a polar aprotic solvent was added. After mixing evenly, stirring was continued for 2 hours, and the stirring polymerization temperature was kept not exceeding room temperature. The obtained polyamic acid was coated on a stainless steel substrate, and placed in an oven for high-temperature curing to obtain a high-temperature resistant thermoplastic polyimide coating.

[0062] Comparative Example 1, Preparation of coating

[0063] Under nitrogen protection, 225.246 g (1 mol) of 2-(4-aminophenyl)-5-aminobenzoxazole (AAB) was dissolved in 2300 g of DMAc at room temperature, and 236.13 g (1 mol) of pyromellitic dianhydride (PMDA) was added in four batches. After stirring for 6 hours, an amino-terminated silane coupling agent uniformly dispersed in a polar aprotic solvent was not added, and the stirring polymerization temperature was kept at no more than room temperature. The obtained polyamic acid was coated on a stainless steel substrate and placed in an oven for high-temperature curing to obtain a thermoplastic polyimide coating.

[0064] Comparative Example 2, Preparation of Coating

[0065] Under nitrogen protection, 225.246 g (1 mol) of 2-(4-aminophenyl)-5-aminobenzoxazole (AAB) was dissolved in 2300 g of DMAc at room temperature, and 236.13 g (1 mol) of pyromellitic dianhydride (PMDA) was added in four batches. After stirring for 6 hours, 10% wt of γ-aminopropyltrimethoxysilane uniformly dispersed in a polar aprotic solvent was added, and the mixture was mixed and stirred for 2 hours. The obtained polyamic acid was coated on a stainless steel substrate and placed in an oven for high-temperature curing to obtain a thermoplastic polyimide coating.

[0066] Comparative Example 3, Preparation of Coating

[0067] Under nitrogen protection, 225.246 g (1 mol) of 2-(4-aminophenyl)-5-aminobenzoxazole (AAB) was dissolved in 2300 g of DMAc at room temperature, and 236.13 g (1 mol) of pyromellitic dianhydride (PMDA) was added in four batches. After stirring for 6 hours, 1% wt of non-terminated amino silane coupling agent 1,2-bis(triethoxysilyl)ethane uniformly dispersed in a polar aprotic solvent was added. After mixing evenly, stirring was continued for 2 hours, and the stirring polymerization temperature was kept at no more than room temperature. After mixing evenly, it was coated on a stainless steel substrate and placed in an oven for high-temperature curing to obtain a thermoplastic polyimide coating.

[0068] The coatings of Examples 1-5 and Comparative Examples 1-2 were subjected to adhesion tests according to GB / T 9286-1998. The test results are shown in Figure 3 and Figure 4 The glass transition temperature was tested by differential scanning calorimetry, and a high temperature resistance test was carried out in a muffle furnace. The test results are shown in Table 1 below.

[0069] Table 1 Performance test results of the products of Examples 1-5 and Comparative Examples 1-2

[0070]

[0071] As can be seen from the data in Table 1, Examples 1-5 are high temperature resistant coatings end-capped with amino-terminated silane coupling agents, with excellent thermal stability performance data, no cracking at 450°C for 5h, and adhesion levels of 0, with excellent adhesion strength. Comparative Example 1 is a coating that is not end-capped with amino-terminated silane coupling agents. Although the thermal stability performance data is excellent, it cannot be well adhered to the inorganic substrate, the adhesion is poor, and cracking occurs at room temperature, and the protective effect of the coating cannot be achieved, and it has no practical significance. Comparative Example 2 adds an excessive amount of amino-terminated silane coupling agent, and obvious blistering and cracking occur after high-temperature ablation, and the adhesion decreases significantly and the coating protection effect is lost, indicating that it is very necessary to introduce amino-terminated silane coupling agent end-capping into the polyimide coating. However, the silane coupling agent contains a long silane chain, and when the content is added too much, it will affect the stability of the coating structure and reduce the high temperature resistance of the material, and a large amount of coupling agents that do not react with polyamic acid are attached to the inorganic substrate, which will cause the coating adhesion to decrease. Comparative Example 3 adds a non-terminated amino silane coupling agent, which cannot bond with the polyimide main chain and disrupts the regularity of the material molecular structure, resulting in reduced material adhesion. At room temperature, cracking occurs and the protective effect cannot be achieved. However, the silanol produced by the hydrolysis of the appropriately added terminal amino silane coupling agent can bond well with the inorganic substrate, so that a chemical bond is generated between the inorganic substrate and the polyimide coating, which greatly enhances the adhesion strength of the coating and makes the coating truly practical. The preparation process is simple to operate and easy to industrialize, and is expected to further expand the application of polyimide (PI) coatings in the field of thermal protection.

[0072] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A method for preparing a high temperature resistant coating terminated with an amino-terminated silane coupling agent, It is characterized in that The following steps are involved: S1: Under nitrogen protection, diamine is dissolved in a polar aprotic solvent to prepare a diamine solution with a concentration of 20%wt; S2: adding dianhydride to the diamine solution in multiple portions, mixing and reacting for more than 6 hours to obtain polyamic acid; S3: adding an amino-terminated silane coupling agent to the polyamic acid, and continuing the reaction for more than 2 hours to obtain a high temperature resistant coating capped with an amino-terminated silane coupling agent.

2. The method for preparing the high temperature resistant coating terminated by amino-terminated silane coupling agent according to claim 1, It is characterized in that The step S3 specifically includes: adding the amino-terminated silane coupling agent to the polar aprotic solvent, dissolving and dispersing for more than 20 minutes to obtain an amino-terminated silane coupling agent solution, dropping the amino-terminated silane coupling agent solution into the polyamic acid, and continuing the reaction for more than 2 hours to obtain the high-temperature resistant coating capped with the amino-terminated silane coupling agent.

3. The method for preparing the high temperature resistant coating terminated by amino-terminated silane coupling agent according to claim 1, It is characterized in that The polar aprotic solvent is any one of N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP) and dimethyl sulfoxide (DMSO).

4. The method for preparing the high temperature resistant coating terminated by amino-terminated silane coupling agent according to claim 1, It is characterized in that The diamine is one or more of 2-(4-aminophenyl)-5-aminobenzoxazole, 9,9-bis(3-fluoro-4-aminophenyl)fluorene, and 2,2'-bis(trifluoromethyl)-(1,1'-diphenyl)-4,4'-diamine.

5. The method for preparing the high temperature resistant coating terminated by amino-terminated silane coupling agent according to claim 1, It is characterized in that The dianhydride is an aromatic dianhydride, and the aromatic dianhydride is one or more of 2,3,3',4'-biphenyltetracarboxylic dianhydride, pyromellitic dianhydride or hexafluoro dianhydride.

6. The method for preparing the high temperature resistant coating terminated by amino-terminated silane coupling agent according to claim 1, It is characterized in that The amino-terminated silane coupling agent is one or more of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldiethoxysilane or γ-aminopropylmethyldimethoxysilane.

7. The method for preparing the high temperature resistant coating terminated with amino-terminated silane coupling agent according to claim 1, It is characterized in that The added amount of the amino-terminated silane coupling agent is 1%-5% of the total solid mass of the diamine and the dianhydride.

8. The method for preparing the high temperature resistant coating terminated with amino-terminated silane coupling agent according to claim 1, It is characterized in that The molar ratio of the added amounts of the diamine and the dianhydride is 1:

1.

9. A high temperature resistant coating terminated with an amino-terminated silane coupling agent, It is characterized in that The high temperature resistant coating is prepared by the preparation method of the amino-terminated silane coupling agent-capped high temperature resistant coating as described in any one of claims 1 to 8.

10. An application of the high temperature resistant coating terminated with an amino-terminated silane coupling agent as claimed in claim 9, It is characterized in that Apply it on the stainless steel plate and put it into the oven for high temperature curing.

Citation Information

Patent Citations

  • Method for preparing polyimide coating adhesive with high adhesive force

    CN104945626A

  • Preparation method for colorless transparent high-temperature-resistant polyimide nanometer composite film

    CN105440284A

  • Polyimide paint for enameled wire with high heat resistant grade

    CN105524546A

  • High-voltage-resistant and corona-resistant polyimide insulating paint material and preparation method thereof

    CN116162407A

  • Multipurpose high-temperature-resistant inorganic nano hybrid polyimide resin coating adhesive and preparation method thereof

    CN116790184A